Steel for forming
Our metallic coated forming steels are available in a wide range of grades and corrosion-resistant coatings. Each grade is designed for specific applications and comes with a choice of surface quality. Extensive dimensional choice provides opportunities for cutting waste and maximising yield.
MagiZinc® improves corrosion resistance with half the thickness of conventional zinc coatings, increasing yield, reducing cost and facilitating stronger, lighter products. It offers improved automotive corrosion protection and higher process efficiency.
Applications
- Automotive components
- Building components
- Domestic appliances
- Electrical goods
- Tubes and sections
EN-Engineering-Product-Metallic coated-Forming-DX51D+Z/+ZF/+ZM TSE
EN-Engineering-Product-Metallic coated-Forming-All Grades OverviewTSE
Overview
With MagiZinc® you can manufacture lighter products with higher strength thanks to the improved corrosion protection and at the same time increase the production volume and further reduce costs thanks to the better processing properties.
Relationship with standards
Metallic coated steel for forming complies with the following European standard
EN 10346: 2015 |
---|
DX51D+Z/+ZF/+ZM |
DX52D+Z/+ZF/+ZM |
DX53D+Z/+ZF/+ZM |
DX54D+Z/+ZF/+ZM |
DX56D+Z/+ZF/+ZM |
DX57D+Z/+ZM |
DX58D+Z 1 |
1. Not in standard. Tata Steel’s own specification.
EN-Engineering-Product-Metallic coated-All Grades Coatings Surface aspectsTSE
Coatings
Three types of metallic coating are available:
Pure zinc
Galvanised steel (+Z) is coated with an almost pure zinc coating (>99% zinc).
Zinc-iron alloy
Galvannealed steel (+ZF) is coated with a zinc coating containing approximately 8-12% iron.
For further information on our galvannealed products please visit our Automotive catalogue.
MagiZinc
MagiZinc steel (+ZM) is coated with a zinc coating containing additional magnesium and aluminium.
Coating weight
Coating | Minimum | Maximum |
---|---|---|
Pure zinc (Z) | 90 (6 µm/side) | 600 (42 µm/side) |
Zinc-iron (ZF) | 90 (6 µm/side) | 140 (10 µm/side) |
MagiZinc (ZM)1 | 70 (5 µm/side) | 310 (22 µm/side) |
Coating weight measured in g/m2 double-sided (µm, per side).
Coils with coatings > 450 g/m2 will be supplied in oscillated coiled condition.
Coils coated with 600 g/m2 are only available in width range 980 to 1300 mm.
1 For MagiZinc (ZM) coating weights below 100 g/m2 please visit our Automotive catalogue.
Surface quality
Surface quality complies with standard: EN 10346:2015. Galvanised steels are available in surface quality A, B or C.
For the highest surface quality requirements we also offer Serica FLO®. For more details please visit our Automotive catalogue.
Surface quality A: as coated surface
Imperfections such as pimples, marks, scratches, pits, variations in surface appearance, dark spots, stripe marks and light passivation stains are permissible.
Stretch levelling breaks or run-off marks may appear. Coil breaks and stretcher strains may also appear.
Surface quality B: improved surface
With this surface quality, small imperfections such as stretch levelling breaks, skin pass marks, slight scratches, indentations, surface structure, zinc run-off marks and light passivation stains are permissible.
Surface quality C: best quality surface
Surface condition C is obtained by skin passing. The controlled surface shall make it possible to apply a uniform high-class paint finish. The other surface shall at least have the characteristics of surface quality B.
Surface finish
Pure zinc
MA: minimised spangle, as coated surface (Z).
MB: minimised spangle, improved surface (Z).
MC: minimised spangle, best quality surface (Z).
Zinc-iron alloy
A: as coated surface (ZF).
B: improved surface (ZF).
C: best quality surface (ZF).
MagiZinc®
A : as coated surface (ZM).
B : improved surface (ZM).
C: best quality surface (ZM).
Surface roughness
Metallic coated steel (with the exception of galvanised steel with standard surface (MA)) can be supplied in various grades of roughness – please contact us for more details. If no roughness is specified, roughness will be as shown in the table below.
Roughness Ra (µm) |
|
---|---|
cut off 0.8mm | cut off 2.5mm |
0.6 - 1.9 | 0.7 - 2.2 |
Surface treatments
The surface treatments available are O, C and CO.
Oiling (O)
The material surface can be oiled with preservative oil. Other types of oil - for increasing strength or reducing weight – are available to help achieve your optimum performance parameters. Please contact us for details.
Tata Steel offers the following range of oiling levels:
Coating type | Capability |
---|---|
Pure zinc (Z) | 0.25 - 1.5 g/m2 |
Zinc-iron (ZF) | 0.5 - 1.5 g/m2 |
MagiZinc® (ZM) | 0.25 - 1.5 g/m2 |
Other oiling levels are available on request.
Chromium-free passivation (C)
This surface treatment temporarily protects the zinc-coated material against white rust during transportation and storage (not applicable to all qualities and dimensions – please contact us for details).
Chromium-free passivation and oiled (CO)
Please request this combination of surface treatments if you require extra protection against white rust formation (not applicable to all qualities and dimensions – please contact us for details).
Untreated (U)
Please contact us regarding the availability of untreated coils.
T-treatment
Please contact us for further information.
Prime Lubrication Treatment (PLT)
Prime Lubrication Treatment facilitates the manufacturing of stamped components by minimising known issues in stamping and joining.
For further information please visit our Prime Lubrication Treatment (PLT) page.
EN-Engineering-Product-Metallic coated-Forming-DX51D-PropertiesTSE
Properties
Mechanical properties
Metallic coated steel for forming has the following mechanical properties. These are measured transverse to the rolling direction:
EN 10346: 2015 | Grade | DX51D+Z/+ZF/+ZM |
---|---|---|
Yield strength 1 Re | N/mm² | - |
Tensile strength Rm | N/mm² | 270 - 500 |
Min. elongation 2 | % | 22 |
Min. r-value | - | |
Min. n-value | - |
1. If the yield point is not pronounced, the values apply to the 0.2% - proof strength Rp0.2 ;
if the yield strength is pronounced, the values apply to the lower yield point ReL.
2. Decreased minimum elongation values apply for product thickness t ≤ 0.50mm (minus 4 units) and for 0.50mm ≤ t ≤ 0.70mm (minus 2 units).
Elongation after fracture A uses test piece length L0 = 80 mm.
Chemical composition
Tata Steel complies with the following cast analysis:
EN 10346: 2015 | Grade | DX51D+Z/+ZF/+ZM |
---|---|---|
C | Max. | 0.18 |
Mn | Max. | 1.20 |
P | Max. | 0.12 |
S | Max. | 0.045 |
SI | Max. | 0.50 |
Ti | Max. | 0.30 |
All values are in weight%.
EN-Engineering-Product-Metallic coated-Forming-DX51D-DimensionsTSE
Dimensional capability
Galvanised (+Z) products
Dimensions in mm.
Thickness | Max. width |
---|---|
From - up to | DX51D |
0.35 - 0.40 | 1370 |
0.40 - 0.55 | 1520 |
0.55 - 0.60 | 1600 |
0.60 - 0.65 | 1770 |
0.65 - 0.70 | 1870 |
0.70 - 0.75 | 1890 |
0.75 - 0.80 | 1990 |
0.80 - 2.00 | 2000 |
2.00 - 2.50 | 1550 |
2.50 - 3.50 | 1540 |
3.50 - 3.60 | 1500 |
3.60 - 3.70 | 1450 |
3.70 - 3.85 | 1400 |
3.85 - 4.00 | 1350 |
For widths below 1000 mm, please contact us.
For thicknesses over 2.50 mm, the minimum width is 1000 mm.
Galvannealed (+ZF) products
Dimensions in mm.
Thickness | Max. width |
---|---|
From - up to | DX51D |
0.50 - 0.60 | 1420 |
0.60 - 0.65 | 1700 |
0.65 - 1.50 | 1850 |
1.50 - 1.60 | 1830 |
1.60 - 1.70 | 1710 |
1.70 - 1.75 | 1660 |
1.75 - 1.80 | 1620 |
1.80 - 1.90 | 1530 |
1.90 - 2.00 | 1440 |
For widths below 1000 mm, please contact us.
MagiZinc® (+ZM) products
Dimensions in mm.
Thickness | Max. width |
---|---|
From - up to | DX51D |
0.40 - 0.55 | 1520 |
0.55 - 0.60 | 1600 |
0.60 - 0.65 | 1770 |
0.65 - 0.70 | 1870 |
0.70 - 0.75 | 1890 |
0.75 - 0.80 | 1990 |
0.80 - 2.00 | 2000 |
For widths below 1000 mm, please contact us.
For thicknesses between 2.00 and 2.50 mm, please contact us.
Tolerances
Tolerances comply with standard EN 10143 2006.
Tighter tolerances are available, please contact us for details.
EN-EngineeringAutomotive-Product-Metallic Coated-All Grades Shape and Dimensional TolerancesTSE
Tolerances on thickness
The tolerances comply with standard EN 10143: 2006.
Tighter tolerances are available on request.
Thickness tolerance availability is shown below:
Thickness tolerance | Availability |
---|---|
Full thickness tolerance | Available |
Special thickness tolerance | Available |
50% of full thickness tolerance | Refer before ordering |
The following tolerances apply to the grades with a minimum value for the
yield strength lower than 260 N/mm².
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
> 0.40 | ≤ 0.60 | ± 0.04 | ± 0.05 | ± 0.06 | ± 0.035 | ± 0.040 | ± 0.045 |
> 0.60 | ≤ 0.80 | ± 0.05 | ± 0.06 | ± 0.07 | ± 0.040 | ± 0.045 | ± 0.050 |
> 0.80 | ≤ 1.00 | ± 0.06 | ± 0.07 | ± 0.08 | ± 0.045 | ± 0.050 | ± 0.060 |
> 1.00 | ≤ 1.20 | ± 0.07 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 1.20 | ≤ 1.60 | ± 0.10 | ± 0.11 | ± 0.12 | ± 0.060 | ± 0.070 | ± 0.080 |
> 1.60 | ≤ 2.00 | ± 0.12 | ± 0.13 | ± 0.14 | ± 0.070 | ± 0.080 | ± 0.090 |
> 2.00 | ≤ 2.50 | ± 0.14 | ± 0.15 | ± 0.16 | ± 0.090 | ± 0.100 | ± 0.110 |
> 2.50 | ≤ 3.00 | ± 0.17 | ± 0.17 | ± 0.18 | ± 0.110 | ± 0.120 | ± 0.130 |
> 3.00 | ≤ 5.00 | ± 0.20 | ± 0.20 | ± 0.21 | ± 0.15 | ± 0.16 | ± 0.17 |
> 5.00 | ≤ 6.50 | ± 0.22 | ± 0.22 | ± 0.23 | ± 0.17 | ± 0.18 | ± 0.19 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02 mm.
The following tolerances apply to the steel grades with a minimum value for the
yield strength 260 N/mm² ≤ Rp0.2 < 360 N/mm² and for grades DX51D and S550GD.
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
≥ 0.35 | ≤ 0.40 | ± 0.05 | ± 0.06 | - | ± 0.035 | ± 0.040 | - |
> 0.40 | ≤ 0.60 | ± 0.05 | ± 0.06 | ± 0.07 | ± 0.040 | ± 0.045 | ± 0.050 |
> 0.60 | ≤ 0.80 | ± 0.06 | ± 0.07 | ± 0.08 | ± 0.045 | ± 0.050 | ± 0.060 |
> 0.80 | ≤ 1.00 | ± 0.07 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 1.00 | ≤ 1.20 | ± 0.08 | ± 0.09 | ± 0.11 | ± 0.060 | ± 0.070 | ± 0.080 |
> 1.20 | ≤ 1.60 | ± 0.11 | ± 0.13 | ± 0.14 | ± 0.070 | ± 0.080 | ± 0.090 |
> 1.60 | ≤ 2.00 | ± 0.14 | ± 0.15 | ± 0.16 | ± 0.080 | ± 0.090 | ± 0.110 |
> 2.00 | ≤ 2.50 | ± 0.16 | ± 0.17 | ± 0.18 | ± 0.110 | ± 0.120 | ± 0.130 |
> 2.50 | ≤ 3.00 | ± 0.19 | ± 0.20 | ± 0.20 | ± 0.130 | ± 0.140 | ± 0.150 |
> 3.00 | ≤ 5.00 | ± 0.22 | ± 0.24 | ± 0.25 | ± 0.17 | ± 0.18 | ± 0.19 |
> 5.00 | ≤ 6.50 | ± 0.24 | ± 0.25 | ± 0.26 | ± 0.19 | ± 0.20 | ± 0.21 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02mm
The following tolerances apply to the steel grades with a minimum value for the
yield strength 360 N/mm² ≤ Rp0.2 ≤ 420 N/mm².
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
≥ 0.35 | ≤ 0.40 | ± 0.05 | ± 0.06 | - | ± 0.040 | ± 0.045 | - |
> 0.40 | ≤ 0.60 | ± 0.06 | ± 0.07 | ± 0.08 | ± 0.045 | ± 0.050 | ± 0.060 |
> 0.60 | ≤ 0.80 | ± 0.07 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 0.80 | ≤ 1.00 | ± 0.08 | ± 0.09 | ± 0.11 | ± 0.060 | ± 0.070 | ± 0.080 |
> 1.00 | ≤ 1.20 | ± 0.10 | ± 0.11 | ± 0.12 | ± 0.070 | ± 0.080 | ± 0.090 |
> 1.20 | ≤ 1.60 | ± 0.13 | ± 0.14 | ± 0.16 | ± 0.080 | ± 0.090 | ± 0.110 |
> 1.60 | ≤ 2.00 | ± 0.16 | ± 0.17 | ± 0.19 | ± 0.090 | ± 0.110 | ± 0.120 |
> 2.00 | ≤ 2.50 | ± 0.18 | ± 0.20 | ± 0.21 | ± 0.120 | ± 0.130 | ± 0.140 |
> 2.50 | ≤ 3.00 | ± 0.22 | ± 0.22 | ± 0.23 | ± 0.140 | ± 0.150 | ± 0.160 |
> 3.00 | ≤ 5.00 | ± 0.22 | ± 0.24 | ± 0.25 | ± 0.17 | ± 0.18 | ± 0.19 |
> 5.00 | ≤ 6.50 | ± 0.24 | ± 0.25 | ± 0.26 | ± 0.19 | ± 0.20 | ± 0.21 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02mm.
The following tolerances apply to the steel grades with a minimum value for the
yield strength 420 N/mm² < Rp0.2 ≤ 900 N/mm².
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
≥ 0.35 | ≤ 0.40 | ± 0.06 | ± 0.07 | - | ± 0.045 | ± 0.050 | - |
> 0.40 | ≤ 0.60 | ± 0.06 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 0.60 | ≤ 0.80 | ± 0.07 | ± 0.09 | ± 0.11 | ± 0.060 | ± 0.070 | ± 0.080 |
> 0.80 | ≤ 1.00 | ± 0.09 | ± 0.11 | ± 0.12 | ± 0.070 | ± 0.080 | ± 0.090 |
> 1.00 | ≤ 1.20 | ± 0.11 | ± 0.13 | ± 0.14 | ± 0.080 | ± 0.090 | ± 0.110 |
> 1.20 | ≤ 1.60 | ± 0.15 | ± 0.16 | ± 0.18 | ± 0.090 | ± 0.110 | ± 0.120 |
> 1.60 | ≤ 2.00 | ± 0.18 | ± 0.19 | ± 0.21 | ± 0.110 | ± 0.120 | ± 0.140 |
> 2.00 | ≤ 2.50 | ± 0.21 | ± 0.22 | ± 0.24 | ± 0.140 | ± 0.150 | ± 0.170 |
> 2.50 | ≤ 3.00 | ± 0.24 | ± 0.25 | ± 0.26 | ± 0.170 | ± 0.180 | ± 0.190 |
> 3.00 | ≤ 5.00 | ± 0.26 | ± 0.27 | ± 0.28 | ± 0.23 | ± 0.24 | ± 0.26 |
> 5.00 | ≤ 6.50 | ± 0.28 | ± 0.29 | ± 0.30 | ± 0.25 | ± 0.26 | ± 0.28 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02mm.
Tolerances on width
The tolerances on width comply with standard EN 10143: 2006
MagiZinc is not included in the standard, but fulfils EN 10143: 2006 requirements.
Tighter tolerances are available on request.
Tolerances in mm.
Nominal width w | Normal tolerances | Special tolerances (S) |
---|---|---|
600 ≤ w ≤ 1200 | 5 0 | 2 0 |
1200 < w ≤ 1500 | 6 0 | 2 0 |
1500 < w ≤ 1800 | 7 0 | 3 0 |
w > 1800 | 8 0 | 3 0 |
Dimensions and coil weights
Description | Availability |
---|---|
Coil diameter inner | 610 mm |
(508 mm available on request) | |
Coil diameter outer | 10/7 x width max |
1000 mm min. | |
2500 mm max. | |
Coil weight | 30t max. |
33t max. available after consultation | |
Coil weight limited by maximum outer diameter | |
Maximum weight allowed by road/rail transport | |
Some products may have different coil weight ranges available | |
Usually a minimum coil weight up to 85% of the maximum coil weight can be requested | |
KIM: width ≤ 1200 mm | 11.7 - 22.7 kg/mm width |
KIM: 1200mm < width ≤ 1700 mm | 11.6 - 21.7 kg/mm width |
KIM: width > 1700 mm | 11.0 kg/mm width and 11.6 - 21.7 kg/mm width |
Minimum tonnage per order | Refer to price list for order quantity details |
Minimum order quantities may apply |
EN-EngineeringAutomotive-Product-Metallic coated-All grades Further processingTSE
Further processing
We have a broad network of Tata Steel service centres across Europe, offering decoiling and slitting services from stock and against short lead times
Light gauge processing
Processing type | Slitting | Decoiling | Blanking |
---|---|---|---|
Thickness range (mm) | 0.2 - 7.0 | 0.3 - 6.0 | 0.3 - 6.0 |
Width range (mm) | 10 - 2050 | 50 - 2600 | 200 - 2600 |
Length range | - | up to 6 m | up to 6 m |
Locations | Netherlands Germany France Spain Sweden Norway Finland |
Netherlands Germany France Spain Sweden Norway Finland |
Netherlands |
For further information please visit our Service Centre webpages.
EN-Engineering-Product-Metallic coated-Forming-DX52D+Z/+ZF/+ZM TSE
EN-Engineering-Product-Metallic coated-Forming-All Grades OverviewTSE
Overview
With MagiZinc® you can manufacture lighter products with higher strength thanks to the improved corrosion protection and at the same time increase the production volume and further reduce costs thanks to the better processing properties.
Relationship with standards
Metallic coated steel for forming complies with the following European standard
EN 10346: 2015 |
---|
DX51D+Z/+ZF/+ZM |
DX52D+Z/+ZF/+ZM |
DX53D+Z/+ZF/+ZM |
DX54D+Z/+ZF/+ZM |
DX56D+Z/+ZF/+ZM |
DX57D+Z/+ZM |
DX58D+Z 1 |
1. Not in standard. Tata Steel’s own specification.
EN-Engineering-Product-Metallic coated-All Grades Coatings Surface aspectsTSE
Coatings
Three types of metallic coating are available:
Pure zinc
Galvanised steel (+Z) is coated with an almost pure zinc coating (>99% zinc).
Zinc-iron alloy
Galvannealed steel (+ZF) is coated with a zinc coating containing approximately 8-12% iron.
For further information on our galvannealed products please visit our Automotive catalogue.
MagiZinc
MagiZinc steel (+ZM) is coated with a zinc coating containing additional magnesium and aluminium.
Coating weight
Coating | Minimum | Maximum |
---|---|---|
Pure zinc (Z) | 90 (6 µm/side) | 600 (42 µm/side) |
Zinc-iron (ZF) | 90 (6 µm/side) | 140 (10 µm/side) |
MagiZinc (ZM)1 | 70 (5 µm/side) | 310 (22 µm/side) |
Coating weight measured in g/m2 double-sided (µm, per side).
Coils with coatings > 450 g/m2 will be supplied in oscillated coiled condition.
Coils coated with 600 g/m2 are only available in width range 980 to 1300 mm.
1 For MagiZinc (ZM) coating weights below 100 g/m2 please visit our Automotive catalogue.
Surface quality
Surface quality complies with standard: EN 10346:2015. Galvanised steels are available in surface quality A, B or C.
For the highest surface quality requirements we also offer Serica FLO®. For more details please visit our Automotive catalogue.
Surface quality A: as coated surface
Imperfections such as pimples, marks, scratches, pits, variations in surface appearance, dark spots, stripe marks and light passivation stains are permissible.
Stretch levelling breaks or run-off marks may appear. Coil breaks and stretcher strains may also appear.
Surface quality B: improved surface
With this surface quality, small imperfections such as stretch levelling breaks, skin pass marks, slight scratches, indentations, surface structure, zinc run-off marks and light passivation stains are permissible.
Surface quality C: best quality surface
Surface condition C is obtained by skin passing. The controlled surface shall make it possible to apply a uniform high-class paint finish. The other surface shall at least have the characteristics of surface quality B.
Surface finish
Pure zinc
MA: minimised spangle, as coated surface (Z).
MB: minimised spangle, improved surface (Z).
MC: minimised spangle, best quality surface (Z).
Zinc-iron alloy
A: as coated surface (ZF).
B: improved surface (ZF).
C: best quality surface (ZF).
MagiZinc®
A : as coated surface (ZM).
B : improved surface (ZM).
C: best quality surface (ZM).
Surface roughness
Metallic coated steel (with the exception of galvanised steel with standard surface (MA)) can be supplied in various grades of roughness – please contact us for more details. If no roughness is specified, roughness will be as shown in the table below.
Roughness Ra (µm) |
|
---|---|
cut off 0.8mm | cut off 2.5mm |
0.6 - 1.9 | 0.7 - 2.2 |
Surface treatments
The surface treatments available are O, C and CO.
Oiling (O)
The material surface can be oiled with preservative oil. Other types of oil - for increasing strength or reducing weight – are available to help achieve your optimum performance parameters. Please contact us for details.
Tata Steel offers the following range of oiling levels:
Coating type | Capability |
---|---|
Pure zinc (Z) | 0.25 - 1.5 g/m2 |
Zinc-iron (ZF) | 0.5 - 1.5 g/m2 |
MagiZinc® (ZM) | 0.25 - 1.5 g/m2 |
Other oiling levels are available on request.
Chromium-free passivation (C)
This surface treatment temporarily protects the zinc-coated material against white rust during transportation and storage (not applicable to all qualities and dimensions – please contact us for details).
Chromium-free passivation and oiled (CO)
Please request this combination of surface treatments if you require extra protection against white rust formation (not applicable to all qualities and dimensions – please contact us for details).
Untreated (U)
Please contact us regarding the availability of untreated coils.
T-treatment
Please contact us for further information.
Prime Lubrication Treatment (PLT)
Prime Lubrication Treatment facilitates the manufacturing of stamped components by minimising known issues in stamping and joining.
For further information please visit our Prime Lubrication Treatment (PLT) page.
EN-Engineering-Product-Metallic coated-Forming-DX52D-PropertiesTSE
Properties
Mechanical properties
Metallic coated steel for forming has the following mechanical properties. These are measured transverse to the rolling direction:
EN 10346: 2015 | Grade | DX52D+Z/+ZF/+ZM |
---|---|---|
Yield strength 1 Re | N/mm² | 140 - 300 3 |
Tensile strength Rm | N/mm² | 270 - 420 |
Elongation 2 | % | 26 |
Min. r-value | - | |
Min. n-value | - |
1. If the yield point is not pronounced, the values apply to the 0.2% - proof strength Rp0.2 ; if the yield strength is pronounced, the values apply to the lower yield point ReL.
2. Decreased minimum elongation values apply for product thickness t ≤ 0.50 mm (minus 4 units) and for 0.50 mm ≤ t ≤ 0.70 mm (minus 2 units).
Elongation after fracture A uses test piece length L0 = 80 mm.
3. This value applies to skin-passed products only (surface qualities B and C).
Chemical composition
Tata Steel complies with the following cast analysis:
EN 10346: 2015 | Grade | DX52D+Z/+ZF/+ZM |
---|---|---|
C | Max. | 0.12 |
Mn | Max. | 0.60 |
P | Max. | 0.10 |
S | Max. | 0.045 |
Si | Max. | 0.50 |
Ti | Max. | 0.30 |
All values are in weight%.
EN-Engineering-Product-Metallic coated-Forming-DX52D-DimensionsTSE
Dimensional capability
Galvanised (+Z) products
Dimensions in mm.
Thickness | Max. width |
---|---|
From - up to | DX52D |
0.36 - 0.40 | 1370 |
0.40 - 0.55 | 1520 |
0.55 - 0.60 | 1600 |
0.60 - 0.65 | 1770 |
0.65 - 0.70 | 1870 |
0.70 - 0.75 | 1890 |
0.75 - 0.80 | 1990 |
0.80 - 2.00 | 2000 |
2.00 - 2.50 | 1550 |
2.50 - 3.50 | 1540 |
3.50 - 3.60 | 1500 |
3.60 - 3.70 | 1450 |
3.70 - 3.85 | 1400 |
3.85 - 4.00 | 1350 |
For widths below 1000 mm, please contact us.
For thicknesses over 2.50 mm, the minimum width is 1000 mm.
Galvannealed (+ZF) products
Dimensions in mm.
Thickness | Max. width |
---|---|
From - up to | DX52D |
0.50 - 0.60 | 1420 |
0.60 - 0.65 | 1700 |
0.65 - 1.50 | 1850 |
1.50 - 1.60 | 1830 |
1.60 - 1.70 | 1710 |
1.70 - 1.75 | 1660 |
1.75 - 1.80 | 1620 |
1.80 - 1.90 | 1530 |
1.90 - 2.00 | 1440 |
For widths below 1000 mm, please contact us.
MagiZinc® (+ZM) products
Dimensions in mm.
Thickness | Max. width |
---|---|
From - up to | DX52D |
0.40 - 0.55 | 1520 |
0.55 - 0.60 | 1600 |
0.60 - 0.65 | 1770 |
0.65 - 0.70 | 1870 |
0.70 - 0.75 | 1890 |
0.75 - 0.80 | 1990 |
0.80 - 2.00 | 2000 |
For widths below 1000 mm, please contact us.
For thicknesses between 2.00 and 2.50 mm, please contact us.
Tolerances
Tolerances comply with standard EN 10143 2006.
Tighter tolerances are available, please contact us for details.
EN-EngineeringAutomotive-Product-Metallic Coated-All Grades Shape and Dimensional TolerancesTSE
Tolerances on thickness
The tolerances comply with standard EN 10143: 2006.
Tighter tolerances are available on request.
Thickness tolerance availability is shown below:
Thickness tolerance | Availability |
---|---|
Full thickness tolerance | Available |
Special thickness tolerance | Available |
50% of full thickness tolerance | Refer before ordering |
The following tolerances apply to the grades with a minimum value for the
yield strength lower than 260 N/mm².
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
> 0.40 | ≤ 0.60 | ± 0.04 | ± 0.05 | ± 0.06 | ± 0.035 | ± 0.040 | ± 0.045 |
> 0.60 | ≤ 0.80 | ± 0.05 | ± 0.06 | ± 0.07 | ± 0.040 | ± 0.045 | ± 0.050 |
> 0.80 | ≤ 1.00 | ± 0.06 | ± 0.07 | ± 0.08 | ± 0.045 | ± 0.050 | ± 0.060 |
> 1.00 | ≤ 1.20 | ± 0.07 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 1.20 | ≤ 1.60 | ± 0.10 | ± 0.11 | ± 0.12 | ± 0.060 | ± 0.070 | ± 0.080 |
> 1.60 | ≤ 2.00 | ± 0.12 | ± 0.13 | ± 0.14 | ± 0.070 | ± 0.080 | ± 0.090 |
> 2.00 | ≤ 2.50 | ± 0.14 | ± 0.15 | ± 0.16 | ± 0.090 | ± 0.100 | ± 0.110 |
> 2.50 | ≤ 3.00 | ± 0.17 | ± 0.17 | ± 0.18 | ± 0.110 | ± 0.120 | ± 0.130 |
> 3.00 | ≤ 5.00 | ± 0.20 | ± 0.20 | ± 0.21 | ± 0.15 | ± 0.16 | ± 0.17 |
> 5.00 | ≤ 6.50 | ± 0.22 | ± 0.22 | ± 0.23 | ± 0.17 | ± 0.18 | ± 0.19 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02 mm.
The following tolerances apply to the steel grades with a minimum value for the
yield strength 260 N/mm² ≤ Rp0.2 < 360 N/mm² and for grades DX51D and S550GD.
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
≥ 0.35 | ≤ 0.40 | ± 0.05 | ± 0.06 | - | ± 0.035 | ± 0.040 | - |
> 0.40 | ≤ 0.60 | ± 0.05 | ± 0.06 | ± 0.07 | ± 0.040 | ± 0.045 | ± 0.050 |
> 0.60 | ≤ 0.80 | ± 0.06 | ± 0.07 | ± 0.08 | ± 0.045 | ± 0.050 | ± 0.060 |
> 0.80 | ≤ 1.00 | ± 0.07 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 1.00 | ≤ 1.20 | ± 0.08 | ± 0.09 | ± 0.11 | ± 0.060 | ± 0.070 | ± 0.080 |
> 1.20 | ≤ 1.60 | ± 0.11 | ± 0.13 | ± 0.14 | ± 0.070 | ± 0.080 | ± 0.090 |
> 1.60 | ≤ 2.00 | ± 0.14 | ± 0.15 | ± 0.16 | ± 0.080 | ± 0.090 | ± 0.110 |
> 2.00 | ≤ 2.50 | ± 0.16 | ± 0.17 | ± 0.18 | ± 0.110 | ± 0.120 | ± 0.130 |
> 2.50 | ≤ 3.00 | ± 0.19 | ± 0.20 | ± 0.20 | ± 0.130 | ± 0.140 | ± 0.150 |
> 3.00 | ≤ 5.00 | ± 0.22 | ± 0.24 | ± 0.25 | ± 0.17 | ± 0.18 | ± 0.19 |
> 5.00 | ≤ 6.50 | ± 0.24 | ± 0.25 | ± 0.26 | ± 0.19 | ± 0.20 | ± 0.21 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02mm
The following tolerances apply to the steel grades with a minimum value for the
yield strength 360 N/mm² ≤ Rp0.2 ≤ 420 N/mm².
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
≥ 0.35 | ≤ 0.40 | ± 0.05 | ± 0.06 | - | ± 0.040 | ± 0.045 | - |
> 0.40 | ≤ 0.60 | ± 0.06 | ± 0.07 | ± 0.08 | ± 0.045 | ± 0.050 | ± 0.060 |
> 0.60 | ≤ 0.80 | ± 0.07 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 0.80 | ≤ 1.00 | ± 0.08 | ± 0.09 | ± 0.11 | ± 0.060 | ± 0.070 | ± 0.080 |
> 1.00 | ≤ 1.20 | ± 0.10 | ± 0.11 | ± 0.12 | ± 0.070 | ± 0.080 | ± 0.090 |
> 1.20 | ≤ 1.60 | ± 0.13 | ± 0.14 | ± 0.16 | ± 0.080 | ± 0.090 | ± 0.110 |
> 1.60 | ≤ 2.00 | ± 0.16 | ± 0.17 | ± 0.19 | ± 0.090 | ± 0.110 | ± 0.120 |
> 2.00 | ≤ 2.50 | ± 0.18 | ± 0.20 | ± 0.21 | ± 0.120 | ± 0.130 | ± 0.140 |
> 2.50 | ≤ 3.00 | ± 0.22 | ± 0.22 | ± 0.23 | ± 0.140 | ± 0.150 | ± 0.160 |
> 3.00 | ≤ 5.00 | ± 0.22 | ± 0.24 | ± 0.25 | ± 0.17 | ± 0.18 | ± 0.19 |
> 5.00 | ≤ 6.50 | ± 0.24 | ± 0.25 | ± 0.26 | ± 0.19 | ± 0.20 | ± 0.21 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02mm.
The following tolerances apply to the steel grades with a minimum value for the
yield strength 420 N/mm² < Rp0.2 ≤ 900 N/mm².
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
≥ 0.35 | ≤ 0.40 | ± 0.06 | ± 0.07 | - | ± 0.045 | ± 0.050 | - |
> 0.40 | ≤ 0.60 | ± 0.06 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 0.60 | ≤ 0.80 | ± 0.07 | ± 0.09 | ± 0.11 | ± 0.060 | ± 0.070 | ± 0.080 |
> 0.80 | ≤ 1.00 | ± 0.09 | ± 0.11 | ± 0.12 | ± 0.070 | ± 0.080 | ± 0.090 |
> 1.00 | ≤ 1.20 | ± 0.11 | ± 0.13 | ± 0.14 | ± 0.080 | ± 0.090 | ± 0.110 |
> 1.20 | ≤ 1.60 | ± 0.15 | ± 0.16 | ± 0.18 | ± 0.090 | ± 0.110 | ± 0.120 |
> 1.60 | ≤ 2.00 | ± 0.18 | ± 0.19 | ± 0.21 | ± 0.110 | ± 0.120 | ± 0.140 |
> 2.00 | ≤ 2.50 | ± 0.21 | ± 0.22 | ± 0.24 | ± 0.140 | ± 0.150 | ± 0.170 |
> 2.50 | ≤ 3.00 | ± 0.24 | ± 0.25 | ± 0.26 | ± 0.170 | ± 0.180 | ± 0.190 |
> 3.00 | ≤ 5.00 | ± 0.26 | ± 0.27 | ± 0.28 | ± 0.23 | ± 0.24 | ± 0.26 |
> 5.00 | ≤ 6.50 | ± 0.28 | ± 0.29 | ± 0.30 | ± 0.25 | ± 0.26 | ± 0.28 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02mm.
Tolerances on width
The tolerances on width comply with standard EN 10143: 2006
MagiZinc is not included in the standard, but fulfils EN 10143: 2006 requirements.
Tighter tolerances are available on request.
Tolerances in mm.
Nominal width w | Normal tolerances | Special tolerances (S) |
---|---|---|
600 ≤ w ≤ 1200 | 5 0 | 2 0 |
1200 < w ≤ 1500 | 6 0 | 2 0 |
1500 < w ≤ 1800 | 7 0 | 3 0 |
w > 1800 | 8 0 | 3 0 |
Dimensions and coil weights
Description | Availability |
---|---|
Coil diameter inner | 610 mm |
(508 mm available on request) | |
Coil diameter outer | 10/7 x width max |
1000 mm min. | |
2500 mm max. | |
Coil weight | 30t max. |
33t max. available after consultation | |
Coil weight limited by maximum outer diameter | |
Maximum weight allowed by road/rail transport | |
Some products may have different coil weight ranges available | |
Usually a minimum coil weight up to 85% of the maximum coil weight can be requested | |
KIM: width ≤ 1200 mm | 11.7 - 22.7 kg/mm width |
KIM: 1200mm < width ≤ 1700 mm | 11.6 - 21.7 kg/mm width |
KIM: width > 1700 mm | 11.0 kg/mm width and 11.6 - 21.7 kg/mm width |
Minimum tonnage per order | Refer to price list for order quantity details |
Minimum order quantities may apply |
EN-EngineeringAutomotive-Product-Metallic coated-All grades Further processingTSE
Further processing
We have a broad network of Tata Steel service centres across Europe, offering decoiling and slitting services from stock and against short lead times
Light gauge processing
Processing type | Slitting | Decoiling | Blanking |
---|---|---|---|
Thickness range (mm) | 0.2 - 7.0 | 0.3 - 6.0 | 0.3 - 6.0 |
Width range (mm) | 10 - 2050 | 50 - 2600 | 200 - 2600 |
Length range | - | up to 6 m | up to 6 m |
Locations | Netherlands Germany France Spain Sweden Norway Finland |
Netherlands Germany France Spain Sweden Norway Finland |
Netherlands |
For further information please visit our Service Centre webpages.
EN-Engineering-Product-Metallic coated-Forming-DX53D+Z/+ZF/+ZM TSE
EN-Engineering-Product-Metallic coated-Forming-All Grades OverviewTSE
Overview
With MagiZinc® you can manufacture lighter products with higher strength thanks to the improved corrosion protection and at the same time increase the production volume and further reduce costs thanks to the better processing properties.
Relationship with standards
Metallic coated steel for forming complies with the following European standard
EN 10346: 2015 |
---|
DX51D+Z/+ZF/+ZM |
DX52D+Z/+ZF/+ZM |
DX53D+Z/+ZF/+ZM |
DX54D+Z/+ZF/+ZM |
DX56D+Z/+ZF/+ZM |
DX57D+Z/+ZM |
DX58D+Z 1 |
1. Not in standard. Tata Steel’s own specification.
EN-Engineering-Product-Metallic coated-All Grades Coatings Surface aspectsTSE
Coatings
Three types of metallic coating are available:
Pure zinc
Galvanised steel (+Z) is coated with an almost pure zinc coating (>99% zinc).
Zinc-iron alloy
Galvannealed steel (+ZF) is coated with a zinc coating containing approximately 8-12% iron.
For further information on our galvannealed products please visit our Automotive catalogue.
MagiZinc
MagiZinc steel (+ZM) is coated with a zinc coating containing additional magnesium and aluminium.
Coating weight
Coating | Minimum | Maximum |
---|---|---|
Pure zinc (Z) | 90 (6 µm/side) | 600 (42 µm/side) |
Zinc-iron (ZF) | 90 (6 µm/side) | 140 (10 µm/side) |
MagiZinc (ZM)1 | 70 (5 µm/side) | 310 (22 µm/side) |
Coating weight measured in g/m2 double-sided (µm, per side).
Coils with coatings > 450 g/m2 will be supplied in oscillated coiled condition.
Coils coated with 600 g/m2 are only available in width range 980 to 1300 mm.
1 For MagiZinc (ZM) coating weights below 100 g/m2 please visit our Automotive catalogue.
Surface quality
Surface quality complies with standard: EN 10346:2015. Galvanised steels are available in surface quality A, B or C.
For the highest surface quality requirements we also offer Serica FLO®. For more details please visit our Automotive catalogue.
Surface quality A: as coated surface
Imperfections such as pimples, marks, scratches, pits, variations in surface appearance, dark spots, stripe marks and light passivation stains are permissible.
Stretch levelling breaks or run-off marks may appear. Coil breaks and stretcher strains may also appear.
Surface quality B: improved surface
With this surface quality, small imperfections such as stretch levelling breaks, skin pass marks, slight scratches, indentations, surface structure, zinc run-off marks and light passivation stains are permissible.
Surface quality C: best quality surface
Surface condition C is obtained by skin passing. The controlled surface shall make it possible to apply a uniform high-class paint finish. The other surface shall at least have the characteristics of surface quality B.
Surface finish
Pure zinc
MA: minimised spangle, as coated surface (Z).
MB: minimised spangle, improved surface (Z).
MC: minimised spangle, best quality surface (Z).
Zinc-iron alloy
A: as coated surface (ZF).
B: improved surface (ZF).
C: best quality surface (ZF).
MagiZinc®
A : as coated surface (ZM).
B : improved surface (ZM).
C: best quality surface (ZM).
Surface roughness
Metallic coated steel (with the exception of galvanised steel with standard surface (MA)) can be supplied in various grades of roughness – please contact us for more details. If no roughness is specified, roughness will be as shown in the table below.
Roughness Ra (µm) |
|
---|---|
cut off 0.8mm | cut off 2.5mm |
0.6 - 1.9 | 0.7 - 2.2 |
Surface treatments
The surface treatments available are O, C and CO.
Oiling (O)
The material surface can be oiled with preservative oil. Other types of oil - for increasing strength or reducing weight – are available to help achieve your optimum performance parameters. Please contact us for details.
Tata Steel offers the following range of oiling levels:
Coating type | Capability |
---|---|
Pure zinc (Z) | 0.25 - 1.5 g/m2 |
Zinc-iron (ZF) | 0.5 - 1.5 g/m2 |
MagiZinc® (ZM) | 0.25 - 1.5 g/m2 |
Other oiling levels are available on request.
Chromium-free passivation (C)
This surface treatment temporarily protects the zinc-coated material against white rust during transportation and storage (not applicable to all qualities and dimensions – please contact us for details).
Chromium-free passivation and oiled (CO)
Please request this combination of surface treatments if you require extra protection against white rust formation (not applicable to all qualities and dimensions – please contact us for details).
Untreated (U)
Please contact us regarding the availability of untreated coils.
T-treatment
Please contact us for further information.
Prime Lubrication Treatment (PLT)
Prime Lubrication Treatment facilitates the manufacturing of stamped components by minimising known issues in stamping and joining.
For further information please visit our Prime Lubrication Treatment (PLT) page.
EN-Engineering-Product-Metallic coated-Forming-DX53D-PropertiesTSE
Properties
Mechanical properties
Metallic coated steel for forming has the following mechanical properties. These are measured transverse to the rolling direction:
EN 10346: 2015 | Grade | DX53D+Z/+ZF/+ZM |
---|---|---|
Yield strength 1 Re | N/mm² | 140 - 260 |
Tensile strength Rm | N/mm² | 270 - 380 |
Elongation 2 | % | 30 |
Min. r-value | - | |
Min. n-value | - |
1. If the yield point is not pronounced, the values apply to the 0.2% - proof strength Rp0.2 ; if the yield strength is pronounced, the values apply to the lower yield point ReL.
2. Decreased minimum elongation values apply for product thickness t ≤ 0.50mm (minus 4 units) and for 0.50mm ≤ t ≤ 0.70mm (minus 2 units).
Elongation after fracture A uses test piece length L0 = 80 mm.
Chemical composition
Tata Steel complies with the following cast analysis:
EN 10346: 2015 | Grade | DX53D+Z/+ZF/+ZM |
---|---|---|
C | Max. | 0.12 |
Mn | Max. | 0.60 |
P | Max. | 0.10 |
S | Max. | 0.045 |
Si | Max. | 0.50 |
Ti | Max. | 0.30 |
All values are in weight%.
EN-Engineering-Product-Metallic coated-Forming-DX53D-DimensionsTSE
Dimensional capability
Galvanised (+Z) products
Dimensions in mm.
Thickness | Max. width |
---|---|
From - up to | DX53D |
0.45 - 0.50 | 1520 |
0.50 - 0.55 | 1540 |
0.55 - 0.60 | 1640 |
0.60 - 0.65 | 1740 |
0.65 - 0.70 | 1830 |
0.70 - 0.75 | 1910 |
0.75 - 0.80 | 1950 |
0.80 - 1.20 | 2000 |
1.20 - 1.30 | 1940 |
1.30 - 1.40 | 1890 |
1.40 - 1.50 | 1830 |
1.50 - 1.60 | 1740 |
1.60 - 1.65 | 1670 |
1.65 - 1.70 | 1640 |
1.70 - 1.75 | 1600 |
1.75 - 1.80 | 1570 |
1.80 - 1.90 | 1530 |
1.90 - 2.00 | 1450 |
For widths below 1000 mm, please contact us.
Galvannealed (+ZF) products
Dimensions in mm.
Thickness | Max. width |
---|---|
From - up to | DX53D |
0.50 - 0.60 | 1420 |
0.60 - 0.65 | 1700 |
0.65 - 1.45 | 1850 |
1.45 - 1.50 | 1850 |
1.50 - 1.60 | 1830 |
1.60 - 1.70 | 1710 |
1.70 - 1.75 | 1660 |
1.75 - 1.80 | 1620 |
1.80 - 1.90 | 1530 |
1.90 - 2.00 | 1440 |
For widths below 1000 mm, please contact us.
MagiZinc® (+ZM) products
Dimensions in mm.
Thickness | Max. width |
---|---|
From - up to | DX53D |
0.45 - 0.50 | 1520 |
0.50 - 0.55 | 1540 |
0.55 - 0.60 | 1640 |
0.60 - 0.65 | 1740 |
0.65 - 0.70 | 1830 |
0.70 - 0.75 | 1910 |
0.75 - 0.80 | 1950 |
0.80 - 1.20 | 2000 |
1.20 - 1.30 | 1940 |
1.30 - 1.40 | 1890 |
1.40 - 1.50 | 1830 |
1.50 - 1.60 | 1740 |
1.60 - 1.70 | 1640 |
1.70 - 1.80 | 1570 |
1.80 - 1.90 | 1530 |
1.90 - 2.00 | 1450 |
For widths below 1000 mm, please contact us.
Tolerances
Tolerances comply with standard EN 10143 2006.
Tighter tolerances are available, please contact us for details.
EN-EngineeringAutomotive-Product-Metallic Coated-All Grades Shape and Dimensional TolerancesTSE
Tolerances on thickness
The tolerances comply with standard EN 10143: 2006.
Tighter tolerances are available on request.
Thickness tolerance availability is shown below:
Thickness tolerance | Availability |
---|---|
Full thickness tolerance | Available |
Special thickness tolerance | Available |
50% of full thickness tolerance | Refer before ordering |
The following tolerances apply to the grades with a minimum value for the
yield strength lower than 260 N/mm².
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
> 0.40 | ≤ 0.60 | ± 0.04 | ± 0.05 | ± 0.06 | ± 0.035 | ± 0.040 | ± 0.045 |
> 0.60 | ≤ 0.80 | ± 0.05 | ± 0.06 | ± 0.07 | ± 0.040 | ± 0.045 | ± 0.050 |
> 0.80 | ≤ 1.00 | ± 0.06 | ± 0.07 | ± 0.08 | ± 0.045 | ± 0.050 | ± 0.060 |
> 1.00 | ≤ 1.20 | ± 0.07 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 1.20 | ≤ 1.60 | ± 0.10 | ± 0.11 | ± 0.12 | ± 0.060 | ± 0.070 | ± 0.080 |
> 1.60 | ≤ 2.00 | ± 0.12 | ± 0.13 | ± 0.14 | ± 0.070 | ± 0.080 | ± 0.090 |
> 2.00 | ≤ 2.50 | ± 0.14 | ± 0.15 | ± 0.16 | ± 0.090 | ± 0.100 | ± 0.110 |
> 2.50 | ≤ 3.00 | ± 0.17 | ± 0.17 | ± 0.18 | ± 0.110 | ± 0.120 | ± 0.130 |
> 3.00 | ≤ 5.00 | ± 0.20 | ± 0.20 | ± 0.21 | ± 0.15 | ± 0.16 | ± 0.17 |
> 5.00 | ≤ 6.50 | ± 0.22 | ± 0.22 | ± 0.23 | ± 0.17 | ± 0.18 | ± 0.19 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02 mm.
The following tolerances apply to the steel grades with a minimum value for the
yield strength 260 N/mm² ≤ Rp0.2 < 360 N/mm² and for grades DX51D and S550GD.
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
≥ 0.35 | ≤ 0.40 | ± 0.05 | ± 0.06 | - | ± 0.035 | ± 0.040 | - |
> 0.40 | ≤ 0.60 | ± 0.05 | ± 0.06 | ± 0.07 | ± 0.040 | ± 0.045 | ± 0.050 |
> 0.60 | ≤ 0.80 | ± 0.06 | ± 0.07 | ± 0.08 | ± 0.045 | ± 0.050 | ± 0.060 |
> 0.80 | ≤ 1.00 | ± 0.07 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 1.00 | ≤ 1.20 | ± 0.08 | ± 0.09 | ± 0.11 | ± 0.060 | ± 0.070 | ± 0.080 |
> 1.20 | ≤ 1.60 | ± 0.11 | ± 0.13 | ± 0.14 | ± 0.070 | ± 0.080 | ± 0.090 |
> 1.60 | ≤ 2.00 | ± 0.14 | ± 0.15 | ± 0.16 | ± 0.080 | ± 0.090 | ± 0.110 |
> 2.00 | ≤ 2.50 | ± 0.16 | ± 0.17 | ± 0.18 | ± 0.110 | ± 0.120 | ± 0.130 |
> 2.50 | ≤ 3.00 | ± 0.19 | ± 0.20 | ± 0.20 | ± 0.130 | ± 0.140 | ± 0.150 |
> 3.00 | ≤ 5.00 | ± 0.22 | ± 0.24 | ± 0.25 | ± 0.17 | ± 0.18 | ± 0.19 |
> 5.00 | ≤ 6.50 | ± 0.24 | ± 0.25 | ± 0.26 | ± 0.19 | ± 0.20 | ± 0.21 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02mm
The following tolerances apply to the steel grades with a minimum value for the
yield strength 360 N/mm² ≤ Rp0.2 ≤ 420 N/mm².
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
≥ 0.35 | ≤ 0.40 | ± 0.05 | ± 0.06 | - | ± 0.040 | ± 0.045 | - |
> 0.40 | ≤ 0.60 | ± 0.06 | ± 0.07 | ± 0.08 | ± 0.045 | ± 0.050 | ± 0.060 |
> 0.60 | ≤ 0.80 | ± 0.07 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 0.80 | ≤ 1.00 | ± 0.08 | ± 0.09 | ± 0.11 | ± 0.060 | ± 0.070 | ± 0.080 |
> 1.00 | ≤ 1.20 | ± 0.10 | ± 0.11 | ± 0.12 | ± 0.070 | ± 0.080 | ± 0.090 |
> 1.20 | ≤ 1.60 | ± 0.13 | ± 0.14 | ± 0.16 | ± 0.080 | ± 0.090 | ± 0.110 |
> 1.60 | ≤ 2.00 | ± 0.16 | ± 0.17 | ± 0.19 | ± 0.090 | ± 0.110 | ± 0.120 |
> 2.00 | ≤ 2.50 | ± 0.18 | ± 0.20 | ± 0.21 | ± 0.120 | ± 0.130 | ± 0.140 |
> 2.50 | ≤ 3.00 | ± 0.22 | ± 0.22 | ± 0.23 | ± 0.140 | ± 0.150 | ± 0.160 |
> 3.00 | ≤ 5.00 | ± 0.22 | ± 0.24 | ± 0.25 | ± 0.17 | ± 0.18 | ± 0.19 |
> 5.00 | ≤ 6.50 | ± 0.24 | ± 0.25 | ± 0.26 | ± 0.19 | ± 0.20 | ± 0.21 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02mm.
The following tolerances apply to the steel grades with a minimum value for the
yield strength 420 N/mm² < Rp0.2 ≤ 900 N/mm².
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
≥ 0.35 | ≤ 0.40 | ± 0.06 | ± 0.07 | - | ± 0.045 | ± 0.050 | - |
> 0.40 | ≤ 0.60 | ± 0.06 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 0.60 | ≤ 0.80 | ± 0.07 | ± 0.09 | ± 0.11 | ± 0.060 | ± 0.070 | ± 0.080 |
> 0.80 | ≤ 1.00 | ± 0.09 | ± 0.11 | ± 0.12 | ± 0.070 | ± 0.080 | ± 0.090 |
> 1.00 | ≤ 1.20 | ± 0.11 | ± 0.13 | ± 0.14 | ± 0.080 | ± 0.090 | ± 0.110 |
> 1.20 | ≤ 1.60 | ± 0.15 | ± 0.16 | ± 0.18 | ± 0.090 | ± 0.110 | ± 0.120 |
> 1.60 | ≤ 2.00 | ± 0.18 | ± 0.19 | ± 0.21 | ± 0.110 | ± 0.120 | ± 0.140 |
> 2.00 | ≤ 2.50 | ± 0.21 | ± 0.22 | ± 0.24 | ± 0.140 | ± 0.150 | ± 0.170 |
> 2.50 | ≤ 3.00 | ± 0.24 | ± 0.25 | ± 0.26 | ± 0.170 | ± 0.180 | ± 0.190 |
> 3.00 | ≤ 5.00 | ± 0.26 | ± 0.27 | ± 0.28 | ± 0.23 | ± 0.24 | ± 0.26 |
> 5.00 | ≤ 6.50 | ± 0.28 | ± 0.29 | ± 0.30 | ± 0.25 | ± 0.26 | ± 0.28 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02mm.
Tolerances on width
The tolerances on width comply with standard EN 10143: 2006
MagiZinc is not included in the standard, but fulfils EN 10143: 2006 requirements.
Tighter tolerances are available on request.
Tolerances in mm.
Nominal width w | Normal tolerances | Special tolerances (S) |
---|---|---|
600 ≤ w ≤ 1200 | 5 0 | 2 0 |
1200 < w ≤ 1500 | 6 0 | 2 0 |
1500 < w ≤ 1800 | 7 0 | 3 0 |
w > 1800 | 8 0 | 3 0 |
Dimensions and coil weights
Description | Availability |
---|---|
Coil diameter inner | 610 mm |
(508 mm available on request) | |
Coil diameter outer | 10/7 x width max |
1000 mm min. | |
2500 mm max. | |
Coil weight | 30t max. |
33t max. available after consultation | |
Coil weight limited by maximum outer diameter | |
Maximum weight allowed by road/rail transport | |
Some products may have different coil weight ranges available | |
Usually a minimum coil weight up to 85% of the maximum coil weight can be requested | |
KIM: width ≤ 1200 mm | 11.7 - 22.7 kg/mm width |
KIM: 1200mm < width ≤ 1700 mm | 11.6 - 21.7 kg/mm width |
KIM: width > 1700 mm | 11.0 kg/mm width and 11.6 - 21.7 kg/mm width |
Minimum tonnage per order | Refer to price list for order quantity details |
Minimum order quantities may apply |
EN-EngineeringAutomotive-Product-Metallic coated-All grades Further processingTSE
Further processing
We have a broad network of Tata Steel service centres across Europe, offering decoiling and slitting services from stock and against short lead times
Light gauge processing
Processing type | Slitting | Decoiling | Blanking |
---|---|---|---|
Thickness range (mm) | 0.2 - 7.0 | 0.3 - 6.0 | 0.3 - 6.0 |
Width range (mm) | 10 - 2050 | 50 - 2600 | 200 - 2600 |
Length range | - | up to 6 m | up to 6 m |
Locations | Netherlands Germany France Spain Sweden Norway Finland |
Netherlands Germany France Spain Sweden Norway Finland |
Netherlands |
For further information please visit our Service Centre webpages.
EN-Engineering-Product-Metallic coated-Forming-DX54D+Z/+ZF/+ZM TSE
EN-Engineering-Product-Metallic coated-Forming-All Grades OverviewTSE
Overview
With MagiZinc® you can manufacture lighter products with higher strength thanks to the improved corrosion protection and at the same time increase the production volume and further reduce costs thanks to the better processing properties.
Relationship with standards
Metallic coated steel for forming complies with the following European standard
EN 10346: 2015 |
---|
DX51D+Z/+ZF/+ZM |
DX52D+Z/+ZF/+ZM |
DX53D+Z/+ZF/+ZM |
DX54D+Z/+ZF/+ZM |
DX56D+Z/+ZF/+ZM |
DX57D+Z/+ZM |
DX58D+Z 1 |
1. Not in standard. Tata Steel’s own specification.
EN-Engineering-Product-Metallic coated-All Grades Coatings Surface aspectsTSE
Coatings
Three types of metallic coating are available:
Pure zinc
Galvanised steel (+Z) is coated with an almost pure zinc coating (>99% zinc).
Zinc-iron alloy
Galvannealed steel (+ZF) is coated with a zinc coating containing approximately 8-12% iron.
For further information on our galvannealed products please visit our Automotive catalogue.
MagiZinc
MagiZinc steel (+ZM) is coated with a zinc coating containing additional magnesium and aluminium.
Coating weight
Coating | Minimum | Maximum |
---|---|---|
Pure zinc (Z) | 90 (6 µm/side) | 600 (42 µm/side) |
Zinc-iron (ZF) | 90 (6 µm/side) | 140 (10 µm/side) |
MagiZinc (ZM)1 | 70 (5 µm/side) | 310 (22 µm/side) |
Coating weight measured in g/m2 double-sided (µm, per side).
Coils with coatings > 450 g/m2 will be supplied in oscillated coiled condition.
Coils coated with 600 g/m2 are only available in width range 980 to 1300 mm.
1 For MagiZinc (ZM) coating weights below 100 g/m2 please visit our Automotive catalogue.
Surface quality
Surface quality complies with standard: EN 10346:2015. Galvanised steels are available in surface quality A, B or C.
For the highest surface quality requirements we also offer Serica FLO®. For more details please visit our Automotive catalogue.
Surface quality A: as coated surface
Imperfections such as pimples, marks, scratches, pits, variations in surface appearance, dark spots, stripe marks and light passivation stains are permissible.
Stretch levelling breaks or run-off marks may appear. Coil breaks and stretcher strains may also appear.
Surface quality B: improved surface
With this surface quality, small imperfections such as stretch levelling breaks, skin pass marks, slight scratches, indentations, surface structure, zinc run-off marks and light passivation stains are permissible.
Surface quality C: best quality surface
Surface condition C is obtained by skin passing. The controlled surface shall make it possible to apply a uniform high-class paint finish. The other surface shall at least have the characteristics of surface quality B.
Surface finish
Pure zinc
MA: minimised spangle, as coated surface (Z).
MB: minimised spangle, improved surface (Z).
MC: minimised spangle, best quality surface (Z).
Zinc-iron alloy
A: as coated surface (ZF).
B: improved surface (ZF).
C: best quality surface (ZF).
MagiZinc®
A : as coated surface (ZM).
B : improved surface (ZM).
C: best quality surface (ZM).
Surface roughness
Metallic coated steel (with the exception of galvanised steel with standard surface (MA)) can be supplied in various grades of roughness – please contact us for more details. If no roughness is specified, roughness will be as shown in the table below.
Roughness Ra (µm) |
|
---|---|
cut off 0.8mm | cut off 2.5mm |
0.6 - 1.9 | 0.7 - 2.2 |
Surface treatments
The surface treatments available are O, C and CO.
Oiling (O)
The material surface can be oiled with preservative oil. Other types of oil - for increasing strength or reducing weight – are available to help achieve your optimum performance parameters. Please contact us for details.
Tata Steel offers the following range of oiling levels:
Coating type | Capability |
---|---|
Pure zinc (Z) | 0.25 - 1.5 g/m2 |
Zinc-iron (ZF) | 0.5 - 1.5 g/m2 |
MagiZinc® (ZM) | 0.25 - 1.5 g/m2 |
Other oiling levels are available on request.
Chromium-free passivation (C)
This surface treatment temporarily protects the zinc-coated material against white rust during transportation and storage (not applicable to all qualities and dimensions – please contact us for details).
Chromium-free passivation and oiled (CO)
Please request this combination of surface treatments if you require extra protection against white rust formation (not applicable to all qualities and dimensions – please contact us for details).
Untreated (U)
Please contact us regarding the availability of untreated coils.
T-treatment
Please contact us for further information.
Prime Lubrication Treatment (PLT)
Prime Lubrication Treatment facilitates the manufacturing of stamped components by minimising known issues in stamping and joining.
For further information please visit our Prime Lubrication Treatment (PLT) page.
EN-Engineering-Product-Metallic coated-Forming-DX54D-PropertiesTSE
Properties
Mechanical properties
Metallic coated steel for forming has the following mechanical properties. These are measured transverse to the rolling direction:
EN 10346: 2015 | Grade | DX54D+Z | DX54D+ZF/+ZM |
---|---|---|---|
Yield strength 1 Re | N/mm² | 120 - 220 | 120 - 220 |
Tensile strength Rm | N/mm² | 260 - 350 | 260 - 350 |
Elongation 2 | % | 36 | 34 |
Min. r-value 3 | 1.6 | 1.4 | |
Min. n-value | 0.18 | 0.18 |
1. If the yield point is not pronounced, the values apply to the 0.2% - proof strength Rp0.2 ; if the yield strength is pronounced, the values apply to the lower yield point ReL.
2. Decreased minimum elongation values apply for product thickness t ≤ 0.50 mm (minus 4 units) and for 0.50 mm ≤ t ≤ 0.70 mm (minus 2 units).
Elongation after fracture A uses test piece length L0 = 80 mm.
3. For t > 1.5 mm, the minimum r90 - value reduced by 0.2 applies.
Chemical composition
Tata Steel complies with the following cast analysis:
EN 10346: 2015 | Grade | DX54D+Z/+ZF/+ZM |
---|---|---|
C | Max. | 0.12 |
Mn | Max. | 0.60 |
P | Max. | 0.10 |
S | Max. | 0.045 |
Si | Max. | 0.50 |
Ti | Max. | 0.30 |
All values are in weight%.
EN-Engineering-Product-Metallic coated-Forming-DX54D-DimensionsTSE
Dimensional capability
Galvanised (+Z) products
Dimensions in mm.
Thickness | Max. width |
---|---|
From - up to | DX54D |
0.45 - 0.50 | 1350 |
0.50 - 0.55 | 1520 |
0.55 - 0.60 | 1620 |
0.60 - 0.65 | 1730 |
0.65 - 0.70 | 1870 |
0.70 - 1.00 | 1970 |
1.00 - 1.20 | 1970 |
1.20 - 1.30 | 1940 |
1.30 - 1.60 | 1840 |
1.60 - 1.70 | 1800 |
1.70 - 1.80 | 1750 |
1.80 - 1.90 | 1630 |
1.90 - 2.00 | 1530 |
For widths below 1000 mm, please contact us.
Galvannealed (+ZF) products
Dimensions in mm.
Thickness | Max. width |
---|---|
From - up to | DX54D |
0.50 - 0.60 | 1420 |
0.60 - 0.65 | 1700 |
0.65 - 1.50 | 1850 |
1.50 - 1.60 | 1830 |
1.60 - 1.70 | 1710 |
1.70 - 1.75 | 1660 |
1.75 - 1.80 | 1620 |
1.80 - 1.90 | 1530 |
1.90 - 2.00 | 1440 |
For widths below 1000 mm, please contact us.
MagiZinc® (+ZM) products
Dimensions in mm.
Thickness | Max. width |
---|---|
From - up to | DX54D |
0.45 - 0.50 | 1350 |
0.50 - 0.55 | 1520 |
0.55 - 0.60 | 1620 |
0.60 - 0.65 | 1730 |
0.65 - 0.70 | 1870 |
0.70 - 1.00 | 1970 |
1.00 - 1.20 | 1970 |
1.20 - 1.30 | 1940 |
1.30 - 1.60 | 1840 |
1.60 - 1.70 | 1800 |
1.70 - 1.80 | 1750 |
1.80 - 1.90 | 1630 |
1.90 - 2.00 | 1530 |
For widths below 1000 mm, please contact us.
Tolerances
Tolerances comply with standard EN 10143 2006.
Tighter tolerances are available, please contact us for details.
EN-EngineeringAutomotive-Product-Metallic Coated-All Grades Shape and Dimensional TolerancesTSE
Tolerances on thickness
The tolerances comply with standard EN 10143: 2006.
Tighter tolerances are available on request.
Thickness tolerance availability is shown below:
Thickness tolerance | Availability |
---|---|
Full thickness tolerance | Available |
Special thickness tolerance | Available |
50% of full thickness tolerance | Refer before ordering |
The following tolerances apply to the grades with a minimum value for the
yield strength lower than 260 N/mm².
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
> 0.40 | ≤ 0.60 | ± 0.04 | ± 0.05 | ± 0.06 | ± 0.035 | ± 0.040 | ± 0.045 |
> 0.60 | ≤ 0.80 | ± 0.05 | ± 0.06 | ± 0.07 | ± 0.040 | ± 0.045 | ± 0.050 |
> 0.80 | ≤ 1.00 | ± 0.06 | ± 0.07 | ± 0.08 | ± 0.045 | ± 0.050 | ± 0.060 |
> 1.00 | ≤ 1.20 | ± 0.07 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 1.20 | ≤ 1.60 | ± 0.10 | ± 0.11 | ± 0.12 | ± 0.060 | ± 0.070 | ± 0.080 |
> 1.60 | ≤ 2.00 | ± 0.12 | ± 0.13 | ± 0.14 | ± 0.070 | ± 0.080 | ± 0.090 |
> 2.00 | ≤ 2.50 | ± 0.14 | ± 0.15 | ± 0.16 | ± 0.090 | ± 0.100 | ± 0.110 |
> 2.50 | ≤ 3.00 | ± 0.17 | ± 0.17 | ± 0.18 | ± 0.110 | ± 0.120 | ± 0.130 |
> 3.00 | ≤ 5.00 | ± 0.20 | ± 0.20 | ± 0.21 | ± 0.15 | ± 0.16 | ± 0.17 |
> 5.00 | ≤ 6.50 | ± 0.22 | ± 0.22 | ± 0.23 | ± 0.17 | ± 0.18 | ± 0.19 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02 mm.
The following tolerances apply to the steel grades with a minimum value for the
yield strength 260 N/mm² ≤ Rp0.2 < 360 N/mm² and for grades DX51D and S550GD.
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
≥ 0.35 | ≤ 0.40 | ± 0.05 | ± 0.06 | - | ± 0.035 | ± 0.040 | - |
> 0.40 | ≤ 0.60 | ± 0.05 | ± 0.06 | ± 0.07 | ± 0.040 | ± 0.045 | ± 0.050 |
> 0.60 | ≤ 0.80 | ± 0.06 | ± 0.07 | ± 0.08 | ± 0.045 | ± 0.050 | ± 0.060 |
> 0.80 | ≤ 1.00 | ± 0.07 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 1.00 | ≤ 1.20 | ± 0.08 | ± 0.09 | ± 0.11 | ± 0.060 | ± 0.070 | ± 0.080 |
> 1.20 | ≤ 1.60 | ± 0.11 | ± 0.13 | ± 0.14 | ± 0.070 | ± 0.080 | ± 0.090 |
> 1.60 | ≤ 2.00 | ± 0.14 | ± 0.15 | ± 0.16 | ± 0.080 | ± 0.090 | ± 0.110 |
> 2.00 | ≤ 2.50 | ± 0.16 | ± 0.17 | ± 0.18 | ± 0.110 | ± 0.120 | ± 0.130 |
> 2.50 | ≤ 3.00 | ± 0.19 | ± 0.20 | ± 0.20 | ± 0.130 | ± 0.140 | ± 0.150 |
> 3.00 | ≤ 5.00 | ± 0.22 | ± 0.24 | ± 0.25 | ± 0.17 | ± 0.18 | ± 0.19 |
> 5.00 | ≤ 6.50 | ± 0.24 | ± 0.25 | ± 0.26 | ± 0.19 | ± 0.20 | ± 0.21 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02mm
The following tolerances apply to the steel grades with a minimum value for the
yield strength 360 N/mm² ≤ Rp0.2 ≤ 420 N/mm².
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
≥ 0.35 | ≤ 0.40 | ± 0.05 | ± 0.06 | - | ± 0.040 | ± 0.045 | - |
> 0.40 | ≤ 0.60 | ± 0.06 | ± 0.07 | ± 0.08 | ± 0.045 | ± 0.050 | ± 0.060 |
> 0.60 | ≤ 0.80 | ± 0.07 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 0.80 | ≤ 1.00 | ± 0.08 | ± 0.09 | ± 0.11 | ± 0.060 | ± 0.070 | ± 0.080 |
> 1.00 | ≤ 1.20 | ± 0.10 | ± 0.11 | ± 0.12 | ± 0.070 | ± 0.080 | ± 0.090 |
> 1.20 | ≤ 1.60 | ± 0.13 | ± 0.14 | ± 0.16 | ± 0.080 | ± 0.090 | ± 0.110 |
> 1.60 | ≤ 2.00 | ± 0.16 | ± 0.17 | ± 0.19 | ± 0.090 | ± 0.110 | ± 0.120 |
> 2.00 | ≤ 2.50 | ± 0.18 | ± 0.20 | ± 0.21 | ± 0.120 | ± 0.130 | ± 0.140 |
> 2.50 | ≤ 3.00 | ± 0.22 | ± 0.22 | ± 0.23 | ± 0.140 | ± 0.150 | ± 0.160 |
> 3.00 | ≤ 5.00 | ± 0.22 | ± 0.24 | ± 0.25 | ± 0.17 | ± 0.18 | ± 0.19 |
> 5.00 | ≤ 6.50 | ± 0.24 | ± 0.25 | ± 0.26 | ± 0.19 | ± 0.20 | ± 0.21 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02mm.
The following tolerances apply to the steel grades with a minimum value for the
yield strength 420 N/mm² < Rp0.2 ≤ 900 N/mm².
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
≥ 0.35 | ≤ 0.40 | ± 0.06 | ± 0.07 | - | ± 0.045 | ± 0.050 | - |
> 0.40 | ≤ 0.60 | ± 0.06 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 0.60 | ≤ 0.80 | ± 0.07 | ± 0.09 | ± 0.11 | ± 0.060 | ± 0.070 | ± 0.080 |
> 0.80 | ≤ 1.00 | ± 0.09 | ± 0.11 | ± 0.12 | ± 0.070 | ± 0.080 | ± 0.090 |
> 1.00 | ≤ 1.20 | ± 0.11 | ± 0.13 | ± 0.14 | ± 0.080 | ± 0.090 | ± 0.110 |
> 1.20 | ≤ 1.60 | ± 0.15 | ± 0.16 | ± 0.18 | ± 0.090 | ± 0.110 | ± 0.120 |
> 1.60 | ≤ 2.00 | ± 0.18 | ± 0.19 | ± 0.21 | ± 0.110 | ± 0.120 | ± 0.140 |
> 2.00 | ≤ 2.50 | ± 0.21 | ± 0.22 | ± 0.24 | ± 0.140 | ± 0.150 | ± 0.170 |
> 2.50 | ≤ 3.00 | ± 0.24 | ± 0.25 | ± 0.26 | ± 0.170 | ± 0.180 | ± 0.190 |
> 3.00 | ≤ 5.00 | ± 0.26 | ± 0.27 | ± 0.28 | ± 0.23 | ± 0.24 | ± 0.26 |
> 5.00 | ≤ 6.50 | ± 0.28 | ± 0.29 | ± 0.30 | ± 0.25 | ± 0.26 | ± 0.28 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02mm.
Tolerances on width
The tolerances on width comply with standard EN 10143: 2006
MagiZinc is not included in the standard, but fulfils EN 10143: 2006 requirements.
Tighter tolerances are available on request.
Tolerances in mm.
Nominal width w | Normal tolerances | Special tolerances (S) |
---|---|---|
600 ≤ w ≤ 1200 | 5 0 | 2 0 |
1200 < w ≤ 1500 | 6 0 | 2 0 |
1500 < w ≤ 1800 | 7 0 | 3 0 |
w > 1800 | 8 0 | 3 0 |
Dimensions and coil weights
Description | Availability |
---|---|
Coil diameter inner | 610 mm |
(508 mm available on request) | |
Coil diameter outer | 10/7 x width max |
1000 mm min. | |
2500 mm max. | |
Coil weight | 30t max. |
33t max. available after consultation | |
Coil weight limited by maximum outer diameter | |
Maximum weight allowed by road/rail transport | |
Some products may have different coil weight ranges available | |
Usually a minimum coil weight up to 85% of the maximum coil weight can be requested | |
KIM: width ≤ 1200 mm | 11.7 - 22.7 kg/mm width |
KIM: 1200mm < width ≤ 1700 mm | 11.6 - 21.7 kg/mm width |
KIM: width > 1700 mm | 11.0 kg/mm width and 11.6 - 21.7 kg/mm width |
Minimum tonnage per order | Refer to price list for order quantity details |
Minimum order quantities may apply |
EN-EngineeringAutomotive-Product-Metallic coated-All grades Further processingTSE
Further processing
We have a broad network of Tata Steel service centres across Europe, offering decoiling and slitting services from stock and against short lead times
Light gauge processing
Processing type | Slitting | Decoiling | Blanking |
---|---|---|---|
Thickness range (mm) | 0.2 - 7.0 | 0.3 - 6.0 | 0.3 - 6.0 |
Width range (mm) | 10 - 2050 | 50 - 2600 | 200 - 2600 |
Length range | - | up to 6 m | up to 6 m |
Locations | Netherlands Germany France Spain Sweden Norway Finland |
Netherlands Germany France Spain Sweden Norway Finland |
Netherlands |
For further information please visit our Service Centre webpages.
EN-Engineering-Product-Metallic coated-Forming-DX56D+Z/+ZF/+ZM TSE
EN-Engineering-Product-Metallic coated-Forming-All Grades OverviewTSE
Overview
With MagiZinc® you can manufacture lighter products with higher strength thanks to the improved corrosion protection and at the same time increase the production volume and further reduce costs thanks to the better processing properties.
Relationship with standards
Metallic coated steel for forming complies with the following European standard
EN 10346: 2015 |
---|
DX51D+Z/+ZF/+ZM |
DX52D+Z/+ZF/+ZM |
DX53D+Z/+ZF/+ZM |
DX54D+Z/+ZF/+ZM |
DX56D+Z/+ZF/+ZM |
DX57D+Z/+ZM |
DX58D+Z 1 |
1. Not in standard. Tata Steel’s own specification.
EN-Engineering-Product-Metallic coated-All Grades Coatings Surface aspectsTSE
Coatings
Three types of metallic coating are available:
Pure zinc
Galvanised steel (+Z) is coated with an almost pure zinc coating (>99% zinc).
Zinc-iron alloy
Galvannealed steel (+ZF) is coated with a zinc coating containing approximately 8-12% iron.
For further information on our galvannealed products please visit our Automotive catalogue.
MagiZinc
MagiZinc steel (+ZM) is coated with a zinc coating containing additional magnesium and aluminium.
Coating weight
Coating | Minimum | Maximum |
---|---|---|
Pure zinc (Z) | 90 (6 µm/side) | 600 (42 µm/side) |
Zinc-iron (ZF) | 90 (6 µm/side) | 140 (10 µm/side) |
MagiZinc (ZM)1 | 70 (5 µm/side) | 310 (22 µm/side) |
Coating weight measured in g/m2 double-sided (µm, per side).
Coils with coatings > 450 g/m2 will be supplied in oscillated coiled condition.
Coils coated with 600 g/m2 are only available in width range 980 to 1300 mm.
1 For MagiZinc (ZM) coating weights below 100 g/m2 please visit our Automotive catalogue.
Surface quality
Surface quality complies with standard: EN 10346:2015. Galvanised steels are available in surface quality A, B or C.
For the highest surface quality requirements we also offer Serica FLO®. For more details please visit our Automotive catalogue.
Surface quality A: as coated surface
Imperfections such as pimples, marks, scratches, pits, variations in surface appearance, dark spots, stripe marks and light passivation stains are permissible.
Stretch levelling breaks or run-off marks may appear. Coil breaks and stretcher strains may also appear.
Surface quality B: improved surface
With this surface quality, small imperfections such as stretch levelling breaks, skin pass marks, slight scratches, indentations, surface structure, zinc run-off marks and light passivation stains are permissible.
Surface quality C: best quality surface
Surface condition C is obtained by skin passing. The controlled surface shall make it possible to apply a uniform high-class paint finish. The other surface shall at least have the characteristics of surface quality B.
Surface finish
Pure zinc
MA: minimised spangle, as coated surface (Z).
MB: minimised spangle, improved surface (Z).
MC: minimised spangle, best quality surface (Z).
Zinc-iron alloy
A: as coated surface (ZF).
B: improved surface (ZF).
C: best quality surface (ZF).
MagiZinc®
A : as coated surface (ZM).
B : improved surface (ZM).
C: best quality surface (ZM).
Surface roughness
Metallic coated steel (with the exception of galvanised steel with standard surface (MA)) can be supplied in various grades of roughness – please contact us for more details. If no roughness is specified, roughness will be as shown in the table below.
Roughness Ra (µm) |
|
---|---|
cut off 0.8mm | cut off 2.5mm |
0.6 - 1.9 | 0.7 - 2.2 |
Surface treatments
The surface treatments available are O, C and CO.
Oiling (O)
The material surface can be oiled with preservative oil. Other types of oil - for increasing strength or reducing weight – are available to help achieve your optimum performance parameters. Please contact us for details.
Tata Steel offers the following range of oiling levels:
Coating type | Capability |
---|---|
Pure zinc (Z) | 0.25 - 1.5 g/m2 |
Zinc-iron (ZF) | 0.5 - 1.5 g/m2 |
MagiZinc® (ZM) | 0.25 - 1.5 g/m2 |
Other oiling levels are available on request.
Chromium-free passivation (C)
This surface treatment temporarily protects the zinc-coated material against white rust during transportation and storage (not applicable to all qualities and dimensions – please contact us for details).
Chromium-free passivation and oiled (CO)
Please request this combination of surface treatments if you require extra protection against white rust formation (not applicable to all qualities and dimensions – please contact us for details).
Untreated (U)
Please contact us regarding the availability of untreated coils.
T-treatment
Please contact us for further information.
Prime Lubrication Treatment (PLT)
Prime Lubrication Treatment facilitates the manufacturing of stamped components by minimising known issues in stamping and joining.
For further information please visit our Prime Lubrication Treatment (PLT) page.
EN-Engineering-Product-Metallic coated-Forming-DX56D-PropertiesTSE
Properties
Mechanical properties
Metallic coated steel for forming has the following mechanical properties. These are measured transverse to the rolling direction:
EN 10346: 2015 | Grade | DX56D+Z | DX56D+ZF/+ZM |
---|---|---|---|
Yield strength 1 Re | N/mm² | 120 - 180 | 120 - 180 |
Tensile strength Rm | N/mm² | 260 - 350 | 260 - 350 |
Elongation 2 | % | 39 | 37 |
Min. r-value 3 | 1.9 | 1.7 4 | |
Min. n-value | 0.21 | 0.20 4 |
1. If the yield point is not pronounced, the values apply to the 0.2% - proof strength Rp0.2 ; if the yield strength is pronounced, the values apply to the lower yield point ReL.
2. Decreased minimum elongation values apply for product thickness t ≤ 0.50 mm (minus 4 units) and for 0.50 mm ≤ t ≤ 0.70 mm (minus 2 units).
Elongation after fraction A uses test piece length L0 = 80 mm.
3. For t > 1.5 mm, the minimum r90 - value reduced by 0.2 applies.
4. For t ≤ 0.70 mm, the minimum r90 - value reduced by 0.2 and minimum n90- value reduced by 0.01 apply.
Chemical composition
Tata Steel complies with the following cast analysis:
EN 10346: 2015 | Grade | DX56D+Z/+ZF/+ZM |
---|---|---|
C | Max. | 0.12 |
Mn | Max. | 0.60 |
P | Max. | 0.10 |
S | Max. | 0.045 |
Si | Max. | 0.50 |
Ti | Max. | 0.30 |
All values are in weight%.
EN-Engineering-Product-Metallic coated-Forming-DX56D-DimensionsTSE
Dimensional capability
Galvanised (+Z) products
Dimensions in mm.
Thickness | Max. width |
---|---|
From - up to | DX56D |
0.45 - 0.50 | 1350 |
0.50 - 0.55 | 1500 |
0.55 - 0.60 | 1620 |
0.60 - 0.65 | 1730 |
0.65 - 0.70 | 1870 |
0.70 - 1.20 | 1970 |
1.20 - 1.30 | 1940 |
1.30 - 1.60 | 1840 |
1.60 - 1.70 | 1800 |
1.70 - 1.80 | 1720 |
1.80 - 1.90 | 1630 |
1.90 - 2.00 | 1530 |
For widths below 1000 mm, please contact us.
Galvannealed (+ZF) products
Dimensions in mm.
Thickness | Max. width |
---|---|
From - up to | DX56D |
0.50 - 0.60 | 1420 |
0.60 - 0.65 | 1700 |
0.65 - 1.45 | 1850 |
1.45 - 1.50 | 1800 |
1.50 - 1.60 | 1700 |
1.60 - 1.70 | 1600 |
1.70 - 1.75 | 1550 |
For widths below 1000 mm, please contact us.
MagiZinc® (+ZM) products
Dimensions in mm.
Thickness | Max. width |
---|---|
From - up to | DX56D |
0.45 - 0.50 | 1350 |
0.50 - 0.55 | 1500 |
0.55 - 0.60 | 1620 |
0.60 - 0.65 | 1730 |
0.65 - 0.70 | 1870 |
0.70 - 1.20 | 1970 |
1.20 - 1.30 | 1940 |
1.30 - 1.60 | 1840 |
1.60 - 1.70 | 1800 |
1.70 - 1.80 | 1720 |
1.80 - 1.90 | 1630 |
1.90 - 2.00 | 1530 |
For widths below 1000 mm, please contact us.
Tolerances
Tolerances comply with standard EN 10143 2006.
Tighter tolerances are available, please contact us for details.
EN-EngineeringAutomotive-Product-Metallic Coated-All Grades Shape and Dimensional TolerancesTSE
Tolerances on thickness
The tolerances comply with standard EN 10143: 2006.
Tighter tolerances are available on request.
Thickness tolerance availability is shown below:
Thickness tolerance | Availability |
---|---|
Full thickness tolerance | Available |
Special thickness tolerance | Available |
50% of full thickness tolerance | Refer before ordering |
The following tolerances apply to the grades with a minimum value for the
yield strength lower than 260 N/mm².
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
> 0.40 | ≤ 0.60 | ± 0.04 | ± 0.05 | ± 0.06 | ± 0.035 | ± 0.040 | ± 0.045 |
> 0.60 | ≤ 0.80 | ± 0.05 | ± 0.06 | ± 0.07 | ± 0.040 | ± 0.045 | ± 0.050 |
> 0.80 | ≤ 1.00 | ± 0.06 | ± 0.07 | ± 0.08 | ± 0.045 | ± 0.050 | ± 0.060 |
> 1.00 | ≤ 1.20 | ± 0.07 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 1.20 | ≤ 1.60 | ± 0.10 | ± 0.11 | ± 0.12 | ± 0.060 | ± 0.070 | ± 0.080 |
> 1.60 | ≤ 2.00 | ± 0.12 | ± 0.13 | ± 0.14 | ± 0.070 | ± 0.080 | ± 0.090 |
> 2.00 | ≤ 2.50 | ± 0.14 | ± 0.15 | ± 0.16 | ± 0.090 | ± 0.100 | ± 0.110 |
> 2.50 | ≤ 3.00 | ± 0.17 | ± 0.17 | ± 0.18 | ± 0.110 | ± 0.120 | ± 0.130 |
> 3.00 | ≤ 5.00 | ± 0.20 | ± 0.20 | ± 0.21 | ± 0.15 | ± 0.16 | ± 0.17 |
> 5.00 | ≤ 6.50 | ± 0.22 | ± 0.22 | ± 0.23 | ± 0.17 | ± 0.18 | ± 0.19 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02 mm.
The following tolerances apply to the steel grades with a minimum value for the
yield strength 260 N/mm² ≤ Rp0.2 < 360 N/mm² and for grades DX51D and S550GD.
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
≥ 0.35 | ≤ 0.40 | ± 0.05 | ± 0.06 | - | ± 0.035 | ± 0.040 | - |
> 0.40 | ≤ 0.60 | ± 0.05 | ± 0.06 | ± 0.07 | ± 0.040 | ± 0.045 | ± 0.050 |
> 0.60 | ≤ 0.80 | ± 0.06 | ± 0.07 | ± 0.08 | ± 0.045 | ± 0.050 | ± 0.060 |
> 0.80 | ≤ 1.00 | ± 0.07 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 1.00 | ≤ 1.20 | ± 0.08 | ± 0.09 | ± 0.11 | ± 0.060 | ± 0.070 | ± 0.080 |
> 1.20 | ≤ 1.60 | ± 0.11 | ± 0.13 | ± 0.14 | ± 0.070 | ± 0.080 | ± 0.090 |
> 1.60 | ≤ 2.00 | ± 0.14 | ± 0.15 | ± 0.16 | ± 0.080 | ± 0.090 | ± 0.110 |
> 2.00 | ≤ 2.50 | ± 0.16 | ± 0.17 | ± 0.18 | ± 0.110 | ± 0.120 | ± 0.130 |
> 2.50 | ≤ 3.00 | ± 0.19 | ± 0.20 | ± 0.20 | ± 0.130 | ± 0.140 | ± 0.150 |
> 3.00 | ≤ 5.00 | ± 0.22 | ± 0.24 | ± 0.25 | ± 0.17 | ± 0.18 | ± 0.19 |
> 5.00 | ≤ 6.50 | ± 0.24 | ± 0.25 | ± 0.26 | ± 0.19 | ± 0.20 | ± 0.21 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02mm
The following tolerances apply to the steel grades with a minimum value for the
yield strength 360 N/mm² ≤ Rp0.2 ≤ 420 N/mm².
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
≥ 0.35 | ≤ 0.40 | ± 0.05 | ± 0.06 | - | ± 0.040 | ± 0.045 | - |
> 0.40 | ≤ 0.60 | ± 0.06 | ± 0.07 | ± 0.08 | ± 0.045 | ± 0.050 | ± 0.060 |
> 0.60 | ≤ 0.80 | ± 0.07 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 0.80 | ≤ 1.00 | ± 0.08 | ± 0.09 | ± 0.11 | ± 0.060 | ± 0.070 | ± 0.080 |
> 1.00 | ≤ 1.20 | ± 0.10 | ± 0.11 | ± 0.12 | ± 0.070 | ± 0.080 | ± 0.090 |
> 1.20 | ≤ 1.60 | ± 0.13 | ± 0.14 | ± 0.16 | ± 0.080 | ± 0.090 | ± 0.110 |
> 1.60 | ≤ 2.00 | ± 0.16 | ± 0.17 | ± 0.19 | ± 0.090 | ± 0.110 | ± 0.120 |
> 2.00 | ≤ 2.50 | ± 0.18 | ± 0.20 | ± 0.21 | ± 0.120 | ± 0.130 | ± 0.140 |
> 2.50 | ≤ 3.00 | ± 0.22 | ± 0.22 | ± 0.23 | ± 0.140 | ± 0.150 | ± 0.160 |
> 3.00 | ≤ 5.00 | ± 0.22 | ± 0.24 | ± 0.25 | ± 0.17 | ± 0.18 | ± 0.19 |
> 5.00 | ≤ 6.50 | ± 0.24 | ± 0.25 | ± 0.26 | ± 0.19 | ± 0.20 | ± 0.21 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02mm.
The following tolerances apply to the steel grades with a minimum value for the
yield strength 420 N/mm² < Rp0.2 ≤ 900 N/mm².
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
≥ 0.35 | ≤ 0.40 | ± 0.06 | ± 0.07 | - | ± 0.045 | ± 0.050 | - |
> 0.40 | ≤ 0.60 | ± 0.06 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 0.60 | ≤ 0.80 | ± 0.07 | ± 0.09 | ± 0.11 | ± 0.060 | ± 0.070 | ± 0.080 |
> 0.80 | ≤ 1.00 | ± 0.09 | ± 0.11 | ± 0.12 | ± 0.070 | ± 0.080 | ± 0.090 |
> 1.00 | ≤ 1.20 | ± 0.11 | ± 0.13 | ± 0.14 | ± 0.080 | ± 0.090 | ± 0.110 |
> 1.20 | ≤ 1.60 | ± 0.15 | ± 0.16 | ± 0.18 | ± 0.090 | ± 0.110 | ± 0.120 |
> 1.60 | ≤ 2.00 | ± 0.18 | ± 0.19 | ± 0.21 | ± 0.110 | ± 0.120 | ± 0.140 |
> 2.00 | ≤ 2.50 | ± 0.21 | ± 0.22 | ± 0.24 | ± 0.140 | ± 0.150 | ± 0.170 |
> 2.50 | ≤ 3.00 | ± 0.24 | ± 0.25 | ± 0.26 | ± 0.170 | ± 0.180 | ± 0.190 |
> 3.00 | ≤ 5.00 | ± 0.26 | ± 0.27 | ± 0.28 | ± 0.23 | ± 0.24 | ± 0.26 |
> 5.00 | ≤ 6.50 | ± 0.28 | ± 0.29 | ± 0.30 | ± 0.25 | ± 0.26 | ± 0.28 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02mm.
Tolerances on width
The tolerances on width comply with standard EN 10143: 2006
MagiZinc is not included in the standard, but fulfils EN 10143: 2006 requirements.
Tighter tolerances are available on request.
Tolerances in mm.
Nominal width w | Normal tolerances | Special tolerances (S) |
---|---|---|
600 ≤ w ≤ 1200 | 5 0 | 2 0 |
1200 < w ≤ 1500 | 6 0 | 2 0 |
1500 < w ≤ 1800 | 7 0 | 3 0 |
w > 1800 | 8 0 | 3 0 |
Dimensions and coil weights
Description | Availability |
---|---|
Coil diameter inner | 610 mm |
(508 mm available on request) | |
Coil diameter outer | 10/7 x width max |
1000 mm min. | |
2500 mm max. | |
Coil weight | 30t max. |
33t max. available after consultation | |
Coil weight limited by maximum outer diameter | |
Maximum weight allowed by road/rail transport | |
Some products may have different coil weight ranges available | |
Usually a minimum coil weight up to 85% of the maximum coil weight can be requested | |
KIM: width ≤ 1200 mm | 11.7 - 22.7 kg/mm width |
KIM: 1200mm < width ≤ 1700 mm | 11.6 - 21.7 kg/mm width |
KIM: width > 1700 mm | 11.0 kg/mm width and 11.6 - 21.7 kg/mm width |
Minimum tonnage per order | Refer to price list for order quantity details |
Minimum order quantities may apply |
EN-EngineeringAutomotive-Product-Metallic coated-All grades Further processingTSE
Further processing
We have a broad network of Tata Steel service centres across Europe, offering decoiling and slitting services from stock and against short lead times
Light gauge processing
Processing type | Slitting | Decoiling | Blanking |
---|---|---|---|
Thickness range (mm) | 0.2 - 7.0 | 0.3 - 6.0 | 0.3 - 6.0 |
Width range (mm) | 10 - 2050 | 50 - 2600 | 200 - 2600 |
Length range | - | up to 6 m | up to 6 m |
Locations | Netherlands Germany France Spain Sweden Norway Finland |
Netherlands Germany France Spain Sweden Norway Finland |
Netherlands |
For further information please visit our Service Centre webpages.
EN-Engineering-Product-Metallic coated-Forming-DX57D+Z/+ZM TSE
EN-Engineering-Product-Metallic coated-Forming-All Grades OverviewTSE
Overview
With MagiZinc® you can manufacture lighter products with higher strength thanks to the improved corrosion protection and at the same time increase the production volume and further reduce costs thanks to the better processing properties.
Relationship with standards
Metallic coated steel for forming complies with the following European standard
EN 10346: 2015 |
---|
DX51D+Z/+ZF/+ZM |
DX52D+Z/+ZF/+ZM |
DX53D+Z/+ZF/+ZM |
DX54D+Z/+ZF/+ZM |
DX56D+Z/+ZF/+ZM |
DX57D+Z/+ZM |
DX58D+Z 1 |
1. Not in standard. Tata Steel’s own specification.
EN-Engineering-Product-Metallic coated-All Grades Coatings Surface aspectsTSE
Coatings
Three types of metallic coating are available:
Pure zinc
Galvanised steel (+Z) is coated with an almost pure zinc coating (>99% zinc).
Zinc-iron alloy
Galvannealed steel (+ZF) is coated with a zinc coating containing approximately 8-12% iron.
For further information on our galvannealed products please visit our Automotive catalogue.
MagiZinc
MagiZinc steel (+ZM) is coated with a zinc coating containing additional magnesium and aluminium.
Coating weight
Coating | Minimum | Maximum |
---|---|---|
Pure zinc (Z) | 90 (6 µm/side) | 600 (42 µm/side) |
Zinc-iron (ZF) | 90 (6 µm/side) | 140 (10 µm/side) |
MagiZinc (ZM)1 | 70 (5 µm/side) | 310 (22 µm/side) |
Coating weight measured in g/m2 double-sided (µm, per side).
Coils with coatings > 450 g/m2 will be supplied in oscillated coiled condition.
Coils coated with 600 g/m2 are only available in width range 980 to 1300 mm.
1 For MagiZinc (ZM) coating weights below 100 g/m2 please visit our Automotive catalogue.
Surface quality
Surface quality complies with standard: EN 10346:2015. Galvanised steels are available in surface quality A, B or C.
For the highest surface quality requirements we also offer Serica FLO®. For more details please visit our Automotive catalogue.
Surface quality A: as coated surface
Imperfections such as pimples, marks, scratches, pits, variations in surface appearance, dark spots, stripe marks and light passivation stains are permissible.
Stretch levelling breaks or run-off marks may appear. Coil breaks and stretcher strains may also appear.
Surface quality B: improved surface
With this surface quality, small imperfections such as stretch levelling breaks, skin pass marks, slight scratches, indentations, surface structure, zinc run-off marks and light passivation stains are permissible.
Surface quality C: best quality surface
Surface condition C is obtained by skin passing. The controlled surface shall make it possible to apply a uniform high-class paint finish. The other surface shall at least have the characteristics of surface quality B.
Surface finish
Pure zinc
MA: minimised spangle, as coated surface (Z).
MB: minimised spangle, improved surface (Z).
MC: minimised spangle, best quality surface (Z).
Zinc-iron alloy
A: as coated surface (ZF).
B: improved surface (ZF).
C: best quality surface (ZF).
MagiZinc®
A : as coated surface (ZM).
B : improved surface (ZM).
C: best quality surface (ZM).
Surface roughness
Metallic coated steel (with the exception of galvanised steel with standard surface (MA)) can be supplied in various grades of roughness – please contact us for more details. If no roughness is specified, roughness will be as shown in the table below.
Roughness Ra (µm) |
|
---|---|
cut off 0.8mm | cut off 2.5mm |
0.6 - 1.9 | 0.7 - 2.2 |
Surface treatments
The surface treatments available are O, C and CO.
Oiling (O)
The material surface can be oiled with preservative oil. Other types of oil - for increasing strength or reducing weight – are available to help achieve your optimum performance parameters. Please contact us for details.
Tata Steel offers the following range of oiling levels:
Coating type | Capability |
---|---|
Pure zinc (Z) | 0.25 - 1.5 g/m2 |
Zinc-iron (ZF) | 0.5 - 1.5 g/m2 |
MagiZinc® (ZM) | 0.25 - 1.5 g/m2 |
Other oiling levels are available on request.
Chromium-free passivation (C)
This surface treatment temporarily protects the zinc-coated material against white rust during transportation and storage (not applicable to all qualities and dimensions – please contact us for details).
Chromium-free passivation and oiled (CO)
Please request this combination of surface treatments if you require extra protection against white rust formation (not applicable to all qualities and dimensions – please contact us for details).
Untreated (U)
Please contact us regarding the availability of untreated coils.
T-treatment
Please contact us for further information.
Prime Lubrication Treatment (PLT)
Prime Lubrication Treatment facilitates the manufacturing of stamped components by minimising known issues in stamping and joining.
For further information please visit our Prime Lubrication Treatment (PLT) page.
EN-Engineering-Product-Metallic coated-Forming-DX57D-PropertiesTSE
Properties
Mechanical properties
Metallic coated steel for forming has the following mechanical properties. These are measured transverse to the rolling direction:
EN 10346: 2015 | Grade | DX57D+Z | DX57D+ZM |
---|---|---|---|
Yield strength 1 Re | N/mm² | 120 - 170 | 120 - 170 |
Tensile strength Rm | N/mm² | 260 - 350 | 260 - 350 |
Elongation 2 | % | 41 | 39 |
Min. r-value 3 | 2.1 | 1.9 4 | |
Min. n-value | 0.22 | 0.21 4 |
1. If the yield point is not pronounced, the values apply to the 0.2% - proof strength Rp0.2 ; if the yield strength is pronounced, the values apply to the lower yield point ReL.
2. Decreased minimum elongation values apply for product thickness t ≤ 0.50 mm (minus 4 units) and for 0.50 mm ≤ t ≤ 0.70 mm (minus 2 units).
Elongation after fraction A uses test piece length L0 = 80 mm.
3. For t > 1.5 mm, the minimum r90 - value reduced by 0.2 applies.
4. For t ≤ 0.70 mm, the minimum r90 - value reduced by 0.2 and minimum n90- value reduced by 0.01 apply.
Chemical composition
Tata Steel complies with the following cast analysis:
EN 10346: 2015 | Grade | DX57D+Z/+ZM |
---|---|---|
C | Max. | 0.12 |
Mn | Max. | 0.60 |
P | Max. | 0.10 |
S | Max. | 0.045 |
Si | Max. | 0.50 |
Ti | Max. | 0.30 |
All values are in weight%.
EN-Engineering-Product-Metallic coated-Forming-DX57D-DimensionsTSE
Dimensional capability
Galvanised (+Z) products
Dimensions in mm.
Thickness | Max. width |
---|---|
From - up to | DX57D |
0.50 - 0.55 | 1470 |
0.55 - 0.60 | 1590 |
0.60 - 0.65 | 1710 |
0.65 - 0.70 | 1840 |
0.70 - 0.75 | 1870 |
0.75 - 0.80 | 1900 |
0.80 - 0.90 | 1800 |
0.90 - 1.00 | 1750 |
1.00 - 1.10 | 1600 |
1.10 - 1.20 | 1500 |
For widths below 1000 mm, please contact us.
MagiZinc® (+ZM) products
For the dimensions of DX57D+ZM, please contact us.
Tolerances
Tolerances comply with standard EN 10143 2006.
Tighter tolerances are available, please contact us for details.
EN-EngineeringAutomotive-Product-Metallic Coated-All Grades Shape and Dimensional TolerancesTSE
Tolerances on thickness
The tolerances comply with standard EN 10143: 2006.
Tighter tolerances are available on request.
Thickness tolerance availability is shown below:
Thickness tolerance | Availability |
---|---|
Full thickness tolerance | Available |
Special thickness tolerance | Available |
50% of full thickness tolerance | Refer before ordering |
The following tolerances apply to the grades with a minimum value for the
yield strength lower than 260 N/mm².
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
> 0.40 | ≤ 0.60 | ± 0.04 | ± 0.05 | ± 0.06 | ± 0.035 | ± 0.040 | ± 0.045 |
> 0.60 | ≤ 0.80 | ± 0.05 | ± 0.06 | ± 0.07 | ± 0.040 | ± 0.045 | ± 0.050 |
> 0.80 | ≤ 1.00 | ± 0.06 | ± 0.07 | ± 0.08 | ± 0.045 | ± 0.050 | ± 0.060 |
> 1.00 | ≤ 1.20 | ± 0.07 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 1.20 | ≤ 1.60 | ± 0.10 | ± 0.11 | ± 0.12 | ± 0.060 | ± 0.070 | ± 0.080 |
> 1.60 | ≤ 2.00 | ± 0.12 | ± 0.13 | ± 0.14 | ± 0.070 | ± 0.080 | ± 0.090 |
> 2.00 | ≤ 2.50 | ± 0.14 | ± 0.15 | ± 0.16 | ± 0.090 | ± 0.100 | ± 0.110 |
> 2.50 | ≤ 3.00 | ± 0.17 | ± 0.17 | ± 0.18 | ± 0.110 | ± 0.120 | ± 0.130 |
> 3.00 | ≤ 5.00 | ± 0.20 | ± 0.20 | ± 0.21 | ± 0.15 | ± 0.16 | ± 0.17 |
> 5.00 | ≤ 6.50 | ± 0.22 | ± 0.22 | ± 0.23 | ± 0.17 | ± 0.18 | ± 0.19 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02 mm.
The following tolerances apply to the steel grades with a minimum value for the
yield strength 260 N/mm² ≤ Rp0.2 < 360 N/mm² and for grades DX51D and S550GD.
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
≥ 0.35 | ≤ 0.40 | ± 0.05 | ± 0.06 | - | ± 0.035 | ± 0.040 | - |
> 0.40 | ≤ 0.60 | ± 0.05 | ± 0.06 | ± 0.07 | ± 0.040 | ± 0.045 | ± 0.050 |
> 0.60 | ≤ 0.80 | ± 0.06 | ± 0.07 | ± 0.08 | ± 0.045 | ± 0.050 | ± 0.060 |
> 0.80 | ≤ 1.00 | ± 0.07 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 1.00 | ≤ 1.20 | ± 0.08 | ± 0.09 | ± 0.11 | ± 0.060 | ± 0.070 | ± 0.080 |
> 1.20 | ≤ 1.60 | ± 0.11 | ± 0.13 | ± 0.14 | ± 0.070 | ± 0.080 | ± 0.090 |
> 1.60 | ≤ 2.00 | ± 0.14 | ± 0.15 | ± 0.16 | ± 0.080 | ± 0.090 | ± 0.110 |
> 2.00 | ≤ 2.50 | ± 0.16 | ± 0.17 | ± 0.18 | ± 0.110 | ± 0.120 | ± 0.130 |
> 2.50 | ≤ 3.00 | ± 0.19 | ± 0.20 | ± 0.20 | ± 0.130 | ± 0.140 | ± 0.150 |
> 3.00 | ≤ 5.00 | ± 0.22 | ± 0.24 | ± 0.25 | ± 0.17 | ± 0.18 | ± 0.19 |
> 5.00 | ≤ 6.50 | ± 0.24 | ± 0.25 | ± 0.26 | ± 0.19 | ± 0.20 | ± 0.21 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02mm
The following tolerances apply to the steel grades with a minimum value for the
yield strength 360 N/mm² ≤ Rp0.2 ≤ 420 N/mm².
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
≥ 0.35 | ≤ 0.40 | ± 0.05 | ± 0.06 | - | ± 0.040 | ± 0.045 | - |
> 0.40 | ≤ 0.60 | ± 0.06 | ± 0.07 | ± 0.08 | ± 0.045 | ± 0.050 | ± 0.060 |
> 0.60 | ≤ 0.80 | ± 0.07 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 0.80 | ≤ 1.00 | ± 0.08 | ± 0.09 | ± 0.11 | ± 0.060 | ± 0.070 | ± 0.080 |
> 1.00 | ≤ 1.20 | ± 0.10 | ± 0.11 | ± 0.12 | ± 0.070 | ± 0.080 | ± 0.090 |
> 1.20 | ≤ 1.60 | ± 0.13 | ± 0.14 | ± 0.16 | ± 0.080 | ± 0.090 | ± 0.110 |
> 1.60 | ≤ 2.00 | ± 0.16 | ± 0.17 | ± 0.19 | ± 0.090 | ± 0.110 | ± 0.120 |
> 2.00 | ≤ 2.50 | ± 0.18 | ± 0.20 | ± 0.21 | ± 0.120 | ± 0.130 | ± 0.140 |
> 2.50 | ≤ 3.00 | ± 0.22 | ± 0.22 | ± 0.23 | ± 0.140 | ± 0.150 | ± 0.160 |
> 3.00 | ≤ 5.00 | ± 0.22 | ± 0.24 | ± 0.25 | ± 0.17 | ± 0.18 | ± 0.19 |
> 5.00 | ≤ 6.50 | ± 0.24 | ± 0.25 | ± 0.26 | ± 0.19 | ± 0.20 | ± 0.21 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02mm.
The following tolerances apply to the steel grades with a minimum value for the
yield strength 420 N/mm² < Rp0.2 ≤ 900 N/mm².
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
≥ 0.35 | ≤ 0.40 | ± 0.06 | ± 0.07 | - | ± 0.045 | ± 0.050 | - |
> 0.40 | ≤ 0.60 | ± 0.06 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 0.60 | ≤ 0.80 | ± 0.07 | ± 0.09 | ± 0.11 | ± 0.060 | ± 0.070 | ± 0.080 |
> 0.80 | ≤ 1.00 | ± 0.09 | ± 0.11 | ± 0.12 | ± 0.070 | ± 0.080 | ± 0.090 |
> 1.00 | ≤ 1.20 | ± 0.11 | ± 0.13 | ± 0.14 | ± 0.080 | ± 0.090 | ± 0.110 |
> 1.20 | ≤ 1.60 | ± 0.15 | ± 0.16 | ± 0.18 | ± 0.090 | ± 0.110 | ± 0.120 |
> 1.60 | ≤ 2.00 | ± 0.18 | ± 0.19 | ± 0.21 | ± 0.110 | ± 0.120 | ± 0.140 |
> 2.00 | ≤ 2.50 | ± 0.21 | ± 0.22 | ± 0.24 | ± 0.140 | ± 0.150 | ± 0.170 |
> 2.50 | ≤ 3.00 | ± 0.24 | ± 0.25 | ± 0.26 | ± 0.170 | ± 0.180 | ± 0.190 |
> 3.00 | ≤ 5.00 | ± 0.26 | ± 0.27 | ± 0.28 | ± 0.23 | ± 0.24 | ± 0.26 |
> 5.00 | ≤ 6.50 | ± 0.28 | ± 0.29 | ± 0.30 | ± 0.25 | ± 0.26 | ± 0.28 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02mm.
Tolerances on width
The tolerances on width comply with standard EN 10143: 2006
MagiZinc is not included in the standard, but fulfils EN 10143: 2006 requirements.
Tighter tolerances are available on request.
Tolerances in mm.
Nominal width w | Normal tolerances | Special tolerances (S) |
---|---|---|
600 ≤ w ≤ 1200 | 5 0 | 2 0 |
1200 < w ≤ 1500 | 6 0 | 2 0 |
1500 < w ≤ 1800 | 7 0 | 3 0 |
w > 1800 | 8 0 | 3 0 |
Dimensions and coil weights
Description | Availability |
---|---|
Coil diameter inner | 610 mm |
(508 mm available on request) | |
Coil diameter outer | 10/7 x width max |
1000 mm min. | |
2500 mm max. | |
Coil weight | 30t max. |
33t max. available after consultation | |
Coil weight limited by maximum outer diameter | |
Maximum weight allowed by road/rail transport | |
Some products may have different coil weight ranges available | |
Usually a minimum coil weight up to 85% of the maximum coil weight can be requested | |
KIM: width ≤ 1200 mm | 11.7 - 22.7 kg/mm width |
KIM: 1200mm < width ≤ 1700 mm | 11.6 - 21.7 kg/mm width |
KIM: width > 1700 mm | 11.0 kg/mm width and 11.6 - 21.7 kg/mm width |
Minimum tonnage per order | Refer to price list for order quantity details |
Minimum order quantities may apply |
EN-EngineeringAutomotive-Product-Metallic coated-All grades Further processingTSE
Further processing
We have a broad network of Tata Steel service centres across Europe, offering decoiling and slitting services from stock and against short lead times
Light gauge processing
Processing type | Slitting | Decoiling | Blanking |
---|---|---|---|
Thickness range (mm) | 0.2 - 7.0 | 0.3 - 6.0 | 0.3 - 6.0 |
Width range (mm) | 10 - 2050 | 50 - 2600 | 200 - 2600 |
Length range | - | up to 6 m | up to 6 m |
Locations | Netherlands Germany France Spain Sweden Norway Finland |
Netherlands Germany France Spain Sweden Norway Finland |
Netherlands |
For further information please visit our Service Centre webpages.
EN-Engineering-Product-Metallic coated-Forming-DX58D+Z TSN
EN-Engineering-Product-Metallic coated-Forming-All Grades OverviewTSE
Overview
With MagiZinc® you can manufacture lighter products with higher strength thanks to the improved corrosion protection and at the same time increase the production volume and further reduce costs thanks to the better processing properties.
Relationship with standards
Metallic coated steel for forming complies with the following European standard
EN 10346: 2015 |
---|
DX51D+Z/+ZF/+ZM |
DX52D+Z/+ZF/+ZM |
DX53D+Z/+ZF/+ZM |
DX54D+Z/+ZF/+ZM |
DX56D+Z/+ZF/+ZM |
DX57D+Z/+ZM |
DX58D+Z 1 |
1. Not in standard. Tata Steel’s own specification.
EN-Engineering-Product-Metallic coated-All Grades Coatings Surface aspectsTSE
Coatings
Three types of metallic coating are available:
Pure zinc
Galvanised steel (+Z) is coated with an almost pure zinc coating (>99% zinc).
Zinc-iron alloy
Galvannealed steel (+ZF) is coated with a zinc coating containing approximately 8-12% iron.
For further information on our galvannealed products please visit our Automotive catalogue.
MagiZinc
MagiZinc steel (+ZM) is coated with a zinc coating containing additional magnesium and aluminium.
Coating weight
Coating | Minimum | Maximum |
---|---|---|
Pure zinc (Z) | 90 (6 µm/side) | 600 (42 µm/side) |
Zinc-iron (ZF) | 90 (6 µm/side) | 140 (10 µm/side) |
MagiZinc (ZM)1 | 70 (5 µm/side) | 310 (22 µm/side) |
Coating weight measured in g/m2 double-sided (µm, per side).
Coils with coatings > 450 g/m2 will be supplied in oscillated coiled condition.
Coils coated with 600 g/m2 are only available in width range 980 to 1300 mm.
1 For MagiZinc (ZM) coating weights below 100 g/m2 please visit our Automotive catalogue.
Surface quality
Surface quality complies with standard: EN 10346:2015. Galvanised steels are available in surface quality A, B or C.
For the highest surface quality requirements we also offer Serica FLO®. For more details please visit our Automotive catalogue.
Surface quality A: as coated surface
Imperfections such as pimples, marks, scratches, pits, variations in surface appearance, dark spots, stripe marks and light passivation stains are permissible.
Stretch levelling breaks or run-off marks may appear. Coil breaks and stretcher strains may also appear.
Surface quality B: improved surface
With this surface quality, small imperfections such as stretch levelling breaks, skin pass marks, slight scratches, indentations, surface structure, zinc run-off marks and light passivation stains are permissible.
Surface quality C: best quality surface
Surface condition C is obtained by skin passing. The controlled surface shall make it possible to apply a uniform high-class paint finish. The other surface shall at least have the characteristics of surface quality B.
Surface finish
Pure zinc
MA: minimised spangle, as coated surface (Z).
MB: minimised spangle, improved surface (Z).
MC: minimised spangle, best quality surface (Z).
Zinc-iron alloy
A: as coated surface (ZF).
B: improved surface (ZF).
C: best quality surface (ZF).
MagiZinc®
A : as coated surface (ZM).
B : improved surface (ZM).
C: best quality surface (ZM).
Surface roughness
Metallic coated steel (with the exception of galvanised steel with standard surface (MA)) can be supplied in various grades of roughness – please contact us for more details. If no roughness is specified, roughness will be as shown in the table below.
Roughness Ra (µm) |
|
---|---|
cut off 0.8mm | cut off 2.5mm |
0.6 - 1.9 | 0.7 - 2.2 |
Surface treatments
The surface treatments available are O, C and CO.
Oiling (O)
The material surface can be oiled with preservative oil. Other types of oil - for increasing strength or reducing weight – are available to help achieve your optimum performance parameters. Please contact us for details.
Tata Steel offers the following range of oiling levels:
Coating type | Capability |
---|---|
Pure zinc (Z) | 0.25 - 1.5 g/m2 |
Zinc-iron (ZF) | 0.5 - 1.5 g/m2 |
MagiZinc® (ZM) | 0.25 - 1.5 g/m2 |
Other oiling levels are available on request.
Chromium-free passivation (C)
This surface treatment temporarily protects the zinc-coated material against white rust during transportation and storage (not applicable to all qualities and dimensions – please contact us for details).
Chromium-free passivation and oiled (CO)
Please request this combination of surface treatments if you require extra protection against white rust formation (not applicable to all qualities and dimensions – please contact us for details).
Untreated (U)
Please contact us regarding the availability of untreated coils.
T-treatment
Please contact us for further information.
Prime Lubrication Treatment (PLT)
Prime Lubrication Treatment facilitates the manufacturing of stamped components by minimising known issues in stamping and joining.
For further information please visit our Prime Lubrication Treatment (PLT) page.
EN-Engineering-Product-Metallic coated-Forming-DX58D-PropertiesTSN
Properties
Mechanical properties
Metallic coated steel for forming has the following mechanical properties. These are measured transverse to the rolling direction.
Not in EN 10346: 2015. Tata Steel’s own specification.
Tata Steel | Grade | DX58D+Z |
---|---|---|
Yield strength 1 Re | N/mm² | 120 - 155 |
Tensile strength Rm | N/mm² | 260 - 310 |
Elongation 2 | % | 43 |
Min. r-value | 2.30 | |
Min. n-value | 0.225 |
1. If the yield point is not pronounced, the values apply to the 0.2% - proof strength Rp0.2 ; if the yield strength is pronounced, the values apply to the lower yield point ReL.
2. Decreased minimum elongation values apply for product thickness t ≤ 0.50mm (minus 4 units) and for 0.50mm ≤ t ≤ 0.70mm (minus 2 units).
Elongation after fraction A uses test piece length L0 = 80 mm.
Chemical composition
Tata Steel complies with the following cast analysis:
Tata Steel | Grade | DX58D |
---|---|---|
C | Max. | 0.12 |
Mn | Max. | 0.60 |
P | Max. | 0.10 |
S | Max. | 0.045 |
Si | Max. | 0.50 |
Al | Min. | - |
N | Max. | - |
Ti | Max. | 0.30 |
All values are in weight%.
EN-Engineering-Product-Metallic coated-Forming-DX58D-DimensionsTSN
Dimensional capability
Galvanised (+Z) products
Dimensions in mm.
Thickness | Max. width |
---|---|
From - up to | DX58D |
0.65 - 1.00 | 1820 |
For widths below 1000 mm, please contact us.
Tolerances
Tolerances comply with standard EN 10143 2006.
Tighter tolerances are available, please contact us for details.
EN-EngineeringAutomotive-Product-Metallic Coated-All Grades Shape and Dimensional TolerancesTSE
Tolerances on thickness
The tolerances comply with standard EN 10143: 2006.
Tighter tolerances are available on request.
Thickness tolerance availability is shown below:
Thickness tolerance | Availability |
---|---|
Full thickness tolerance | Available |
Special thickness tolerance | Available |
50% of full thickness tolerance | Refer before ordering |
The following tolerances apply to the grades with a minimum value for the
yield strength lower than 260 N/mm².
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
> 0.40 | ≤ 0.60 | ± 0.04 | ± 0.05 | ± 0.06 | ± 0.035 | ± 0.040 | ± 0.045 |
> 0.60 | ≤ 0.80 | ± 0.05 | ± 0.06 | ± 0.07 | ± 0.040 | ± 0.045 | ± 0.050 |
> 0.80 | ≤ 1.00 | ± 0.06 | ± 0.07 | ± 0.08 | ± 0.045 | ± 0.050 | ± 0.060 |
> 1.00 | ≤ 1.20 | ± 0.07 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 1.20 | ≤ 1.60 | ± 0.10 | ± 0.11 | ± 0.12 | ± 0.060 | ± 0.070 | ± 0.080 |
> 1.60 | ≤ 2.00 | ± 0.12 | ± 0.13 | ± 0.14 | ± 0.070 | ± 0.080 | ± 0.090 |
> 2.00 | ≤ 2.50 | ± 0.14 | ± 0.15 | ± 0.16 | ± 0.090 | ± 0.100 | ± 0.110 |
> 2.50 | ≤ 3.00 | ± 0.17 | ± 0.17 | ± 0.18 | ± 0.110 | ± 0.120 | ± 0.130 |
> 3.00 | ≤ 5.00 | ± 0.20 | ± 0.20 | ± 0.21 | ± 0.15 | ± 0.16 | ± 0.17 |
> 5.00 | ≤ 6.50 | ± 0.22 | ± 0.22 | ± 0.23 | ± 0.17 | ± 0.18 | ± 0.19 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02 mm.
The following tolerances apply to the steel grades with a minimum value for the
yield strength 260 N/mm² ≤ Rp0.2 < 360 N/mm² and for grades DX51D and S550GD.
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
≥ 0.35 | ≤ 0.40 | ± 0.05 | ± 0.06 | - | ± 0.035 | ± 0.040 | - |
> 0.40 | ≤ 0.60 | ± 0.05 | ± 0.06 | ± 0.07 | ± 0.040 | ± 0.045 | ± 0.050 |
> 0.60 | ≤ 0.80 | ± 0.06 | ± 0.07 | ± 0.08 | ± 0.045 | ± 0.050 | ± 0.060 |
> 0.80 | ≤ 1.00 | ± 0.07 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 1.00 | ≤ 1.20 | ± 0.08 | ± 0.09 | ± 0.11 | ± 0.060 | ± 0.070 | ± 0.080 |
> 1.20 | ≤ 1.60 | ± 0.11 | ± 0.13 | ± 0.14 | ± 0.070 | ± 0.080 | ± 0.090 |
> 1.60 | ≤ 2.00 | ± 0.14 | ± 0.15 | ± 0.16 | ± 0.080 | ± 0.090 | ± 0.110 |
> 2.00 | ≤ 2.50 | ± 0.16 | ± 0.17 | ± 0.18 | ± 0.110 | ± 0.120 | ± 0.130 |
> 2.50 | ≤ 3.00 | ± 0.19 | ± 0.20 | ± 0.20 | ± 0.130 | ± 0.140 | ± 0.150 |
> 3.00 | ≤ 5.00 | ± 0.22 | ± 0.24 | ± 0.25 | ± 0.17 | ± 0.18 | ± 0.19 |
> 5.00 | ≤ 6.50 | ± 0.24 | ± 0.25 | ± 0.26 | ± 0.19 | ± 0.20 | ± 0.21 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02mm
The following tolerances apply to the steel grades with a minimum value for the
yield strength 360 N/mm² ≤ Rp0.2 ≤ 420 N/mm².
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
≥ 0.35 | ≤ 0.40 | ± 0.05 | ± 0.06 | - | ± 0.040 | ± 0.045 | - |
> 0.40 | ≤ 0.60 | ± 0.06 | ± 0.07 | ± 0.08 | ± 0.045 | ± 0.050 | ± 0.060 |
> 0.60 | ≤ 0.80 | ± 0.07 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 0.80 | ≤ 1.00 | ± 0.08 | ± 0.09 | ± 0.11 | ± 0.060 | ± 0.070 | ± 0.080 |
> 1.00 | ≤ 1.20 | ± 0.10 | ± 0.11 | ± 0.12 | ± 0.070 | ± 0.080 | ± 0.090 |
> 1.20 | ≤ 1.60 | ± 0.13 | ± 0.14 | ± 0.16 | ± 0.080 | ± 0.090 | ± 0.110 |
> 1.60 | ≤ 2.00 | ± 0.16 | ± 0.17 | ± 0.19 | ± 0.090 | ± 0.110 | ± 0.120 |
> 2.00 | ≤ 2.50 | ± 0.18 | ± 0.20 | ± 0.21 | ± 0.120 | ± 0.130 | ± 0.140 |
> 2.50 | ≤ 3.00 | ± 0.22 | ± 0.22 | ± 0.23 | ± 0.140 | ± 0.150 | ± 0.160 |
> 3.00 | ≤ 5.00 | ± 0.22 | ± 0.24 | ± 0.25 | ± 0.17 | ± 0.18 | ± 0.19 |
> 5.00 | ≤ 6.50 | ± 0.24 | ± 0.25 | ± 0.26 | ± 0.19 | ± 0.20 | ± 0.21 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02mm.
The following tolerances apply to the steel grades with a minimum value for the
yield strength 420 N/mm² < Rp0.2 ≤ 900 N/mm².
Nominal | Normal tolerances for a nominal width of 1 2 | Special tolerances (S) for a | |||||
---|---|---|---|---|---|---|---|
| ≤ 1200 | > 1200 | > 1500 | ≤ 1200 | > 1200 | > 1500 | |
| ≤ 1500 |
|
| ≤ 1500 |
| ||
≥ 0.35 | ≤ 0.40 | ± 0.06 | ± 0.07 | - | ± 0.045 | ± 0.050 | - |
> 0.40 | ≤ 0.60 | ± 0.06 | ± 0.08 | ± 0.09 | ± 0.050 | ± 0.060 | ± 0.070 |
> 0.60 | ≤ 0.80 | ± 0.07 | ± 0.09 | ± 0.11 | ± 0.060 | ± 0.070 | ± 0.080 |
> 0.80 | ≤ 1.00 | ± 0.09 | ± 0.11 | ± 0.12 | ± 0.070 | ± 0.080 | ± 0.090 |
> 1.00 | ≤ 1.20 | ± 0.11 | ± 0.13 | ± 0.14 | ± 0.080 | ± 0.090 | ± 0.110 |
> 1.20 | ≤ 1.60 | ± 0.15 | ± 0.16 | ± 0.18 | ± 0.090 | ± 0.110 | ± 0.120 |
> 1.60 | ≤ 2.00 | ± 0.18 | ± 0.19 | ± 0.21 | ± 0.110 | ± 0.120 | ± 0.140 |
> 2.00 | ≤ 2.50 | ± 0.21 | ± 0.22 | ± 0.24 | ± 0.140 | ± 0.150 | ± 0.170 |
> 2.50 | ≤ 3.00 | ± 0.24 | ± 0.25 | ± 0.26 | ± 0.170 | ± 0.180 | ± 0.190 |
> 3.00 | ≤ 5.00 | ± 0.26 | ± 0.27 | ± 0.28 | ± 0.23 | ± 0.24 | ± 0.26 |
> 5.00 | ≤ 6.50 | ± 0.28 | ± 0.29 | ± 0.30 | ± 0.25 | ± 0.26 | ± 0.28 |
1. Around cold-rolled welds an increase of 20% at the most over the thickness tolerance is allowed
over a length of 15 metres.
2. For zinc coatings ≥ Z450 the tolerance on the thickness must be raised by 0.02mm.
Tolerances on width
The tolerances on width comply with standard EN 10143: 2006
MagiZinc is not included in the standard, but fulfils EN 10143: 2006 requirements.
Tighter tolerances are available on request.
Tolerances in mm.
Nominal width w | Normal tolerances | Special tolerances (S) |
---|---|---|
600 ≤ w ≤ 1200 | 5 0 | 2 0 |
1200 < w ≤ 1500 | 6 0 | 2 0 |
1500 < w ≤ 1800 | 7 0 | 3 0 |
w > 1800 | 8 0 | 3 0 |
Dimensions and coil weights
Description | Availability |
---|---|
Coil diameter inner | 610 mm |
(508 mm available on request) | |
Coil diameter outer | 10/7 x width max |
1000 mm min. | |
2500 mm max. | |
Coil weight | 30t max. |
33t max. available after consultation | |
Coil weight limited by maximum outer diameter | |
Maximum weight allowed by road/rail transport | |
Some products may have different coil weight ranges available | |
Usually a minimum coil weight up to 85% of the maximum coil weight can be requested | |
KIM: width ≤ 1200 mm | 11.7 - 22.7 kg/mm width |
KIM: 1200mm < width ≤ 1700 mm | 11.6 - 21.7 kg/mm width |
KIM: width > 1700 mm | 11.0 kg/mm width and 11.6 - 21.7 kg/mm width |
Minimum tonnage per order | Refer to price list for order quantity details |
Minimum order quantities may apply |
EN-EngineeringAutomotive-Product-Metallic coated-All grades Further processingTSE
Further processing
We have a broad network of Tata Steel service centres across Europe, offering decoiling and slitting services from stock and against short lead times
Light gauge processing
Processing type | Slitting | Decoiling | Blanking |
---|---|---|---|
Thickness range (mm) | 0.2 - 7.0 | 0.3 - 6.0 | 0.3 - 6.0 |
Width range (mm) | 10 - 2050 | 50 - 2600 | 200 - 2600 |
Length range | - | up to 6 m | up to 6 m |
Locations | Netherlands Germany France Spain Sweden Norway Finland |
Netherlands Germany France Spain Sweden Norway Finland |